A porous carbon fiber material with high fracture toughness and preparation method thereof
By combining modified phenolic resin with carbon fiber, porous carbon fiber materials with high fracture toughness are prepared, which solves the problem of fracture of porous carbon materials during the growth of silicon carbide single crystals and improves crystal quality and crystal stability.
Patent Information
- Application Number
- CN202410630484.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-21
AI Technical Summary
Existing porous carbon materials have poor fracture toughness and are prone to fracture due to external pressure during the growth process of silicon carbide single crystal materials, affecting the crystal quality and lattice purity.
Methyltrimethoxysilane and phenolic resin are used for modification. Through the mixing of silicon-modified phenolic resin and carbon fiber during the preparation process, cold pressing mold solidification, carbonization, graphitization and purification, a porous carbon fiber material with high fracture toughness is formed.
It improves the unit fracture toughness of porous carbon fiber materials, reduces the risk of cracks during the fiber growth process, and ensures the ideal crystallization results and the high quality of the crystals.
Smart Images

Figure CN118206392B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous materials, and in particular relates to a porous carbon fiber material with high fracture toughness and a preparation method thereof. Background Art
[0002] Silicon carbide single crystal material is a representative of the third generation of wide bandgap semiconductor materials, with properties such as wide bandgap, high thermal conductivity, high electron saturation mobility, and high breakdown electric field. Compared with semiconductor materials represented by silicon, silicon carbide has obvious advantages and is considered to be an ideal semiconductor material for manufacturing optoelectronic devices, high-frequency and high-power devices, and high-temperature electronic devices. Silicon carbide single crystal materials are widely used in white light lighting, optical storage, screen display, aerospace, high-temperature radiation environment, oil exploration, automation, radar and communication, electric vehicles, and power electronics.
[0003] The growth of silicon carbide single crystal materials is relatively difficult, and physical vapor deposition is currently widely used. The growth process of silicon carbide single crystal materials generally includes: loading silicon carbide source powder into the bottom of the crucible, and fixing silicon carbide seed crystals on the top of the crucible. A porous carbon material is set inside the crucible to separate the silicon carbide source powder and the silicon carbide seed crystals. The porous carbon material contains graphite. During the crystal growth process, the silicon carbide source powder will sublimate after being heated to a certain temperature to form a gas phase substance. These sublimated gas phase substances pass through the porous carbon material and are transported to the surface of the seed crystal to deposit and grow crystals. The porous carbon material is used to separate the silicon carbide source powder and the silicon carbide seed crystal. The pore structure of the porous carbon material can effectively adjust the growth rate of the silicon carbide crystal, reduce the surface defects and grain boundary defects of the silicon carbide crystal, filter the raw material impurities, and improve the crystallization quality and lattice purity. Porous carbon materials can also serve as a support for the growth of silicon carbide crystals, thereby avoiding thermal cracking and deformation of the crystals caused by excessively fast growth rates, and preventing the crystals from deforming or breaking due to their own weight.
[0004] However, the fracture toughness of porous carbon materials in the prior art is generally poor, which results in that during the crystal growth process, the porous carbon materials are easily fractured by external pressure, resulting in unsatisfactory final crystallization results. Summary of the invention
[0005] The purpose of the present invention is to provide a porous carbon fiber material with high fracture toughness that is not prone to breakage during use in order to solve the above problems.
[0006] Another object of the present invention is to provide a method for preparing a porous carbon fiber material with high fracture toughness that is not prone to breakage during use in order to solve the above-mentioned problem.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A porous carbon fiber material with high fracture toughness, wherein the unit fracture toughness of the porous carbon fiber material is 16-22 (MPa•m 1 / 2 *cm 3 ) / g;
[0009] Among them, unit fracture toughness = fracture toughness / density;
[0010] Density: 0.92g / cm 3 ;
[0011] The test standard for fracture toughness is GB / T 23806-2009.
[0012] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 16-17 (MPa•m 1 / 2 *cm 3 ) / g.
[0013] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 17-18 (MPa•m 1 / 2 *cm 3 ) / g.
[0014] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 18-19 (MPa•m 1 / 2 *cm 3 ) / g.
[0015] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 19-20 (MPa•m 1 / 2 *cm 3 ) / g.
[0016] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 20-21 (MPa•m 1 / 2 *cm 3 ) / g.
[0017] In the above-mentioned porous carbon fiber material with high fracture toughness, the unit fracture toughness of the porous carbon fiber material is 21-22 (MPa•m 1 / 2 *cm 3 ) / g.
[0018] A method for preparing the above-mentioned porous carbon fiber material with high fracture toughness comprises the following steps:
[0019] Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 60-80° C. to obtain a mixed solution;
[0020] Step 2: Add oxalic acid to the mixed solution prepared in step 1, stir and heat to 80-100° C., react for 10-14 hours to obtain a reaction solution;
[0021] Step 3: heating the reaction solution obtained in step 2 to 130-140° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0022] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber in a mixer until they are uniformly mixed to obtain a mixture;
[0023] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 150-170℃ for 4-6h;
[0024] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1100-1300°C, the heating rate is 0.4-1°C / min, and the temperature is kept for 30-90 minutes after the heating is completed to obtain a carbon material;
[0025] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2300-2500° C. and a graphitization time of 30-90 min to obtain a graphitized material;
[0026] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2000-2400° C., and the porous carbon material is obtained after the purification process is completed.
[0027] In the above-mentioned method for preparing a porous carbon fiber material with high fracture toughness, the average length of the carbon fiber is 200 microns and the average diameter is 14 microns.
[0028] In the above-mentioned method for preparing a porous carbon fiber material with high fracture toughness, the mass ratio of methyltrimethoxysilane, phenolic resin and oxalic acid is 1:1-1.5:0.005-0.02.
[0029] Compared with the prior art, the advantages of the present invention are:
[0030] 1. The present invention provides a porous carbon fiber material with high unit fracture toughness. During the crystal growth process, the porous carbon fiber material itself, which plays a supporting role, is not easy to break, thereby ensuring the crystallization result.
[0031] 2. The present invention finds that after the phenolic resin is modified with methyltrimethoxysilane, the fiber structure in the carbon material obtained after the phenolic resin is carbonized can be improved to a certain extent in terms of interface, grain boundary and pores, thereby reducing the stress concentration when the fiber is subjected to force, increasing the toughness of the carbon fiber, and at the same time crystallizing inside the fiber to form a smaller crystal core structure, which can deflect or bridge the main crack after the crack occurs, thereby further achieving the effect of improving the fracture toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the SEM image of the porous carbon material prepared in Example 3. DETAILED DESCRIPTION
[0033] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0034] Example 1
[0035] This embodiment provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0036] Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 60° C. to obtain a mixed solution;
[0037] Step 2: adding oxalic acid to the mixed solution prepared in step 1, stirring and heating to 80° C., reacting for 10 hours to obtain a reaction solution, wherein the mass ratio of methyltrimethoxysilane, phenolic resin and oxalic acid is 1:1:0.005;
[0038] Step 3: heating the reaction solution obtained in step 2 to 130° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0039] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0040] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 150℃ for 4h;
[0041] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1100°C, the heating rate is 0.4°C / min, and the temperature is kept for 30 minutes after the heating is completed to obtain a carbon material;
[0042] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2300° C. and a graphitization time of 30 min to obtain a graphitized material;
[0043] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2000° C., and the porous carbon material is obtained after the purification process is completed.
[0044] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0045] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0046] Unit fracture toughness = fracture toughness / density;
[0047] The calculated unit fracture toughness of the porous carbon material is 20.2 (MPa•m 1 / 2 *cm 3 ) / g.
[0048] Example 2
[0049] This embodiment provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0050] Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 80° C. to obtain a mixed solution;
[0051] Step 2: adding oxalic acid to the mixed solution prepared in step 1, stirring and heating to 100° C., reacting for 14 hours to obtain a reaction solution, wherein the mass ratio of methyltrimethoxysilane, phenolic resin and oxalic acid is 1:1.5:0.02;
[0052] Step 3: heating the reaction solution obtained in step 2 to 140° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0053] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0054] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 170℃ for 6h;
[0055] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1300°C, the heating rate is 1°C / min, and the temperature is kept for 90 minutes after the heating is completed to obtain a carbon material;
[0056] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2500° C. and a graphitization time of 90 min to obtain a graphitized material;
[0057] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2400° C., and the porous carbon material is obtained after the purification process is completed.
[0058] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0059] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0060] Unit fracture toughness = fracture toughness / density;
[0061] The calculated unit fracture toughness of the porous carbon material is 20.8 (MPa•m 1 / 2 *cm 3 ) / g.
[0062] Example 3
[0063] This embodiment provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0064] Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 70° C. to obtain a mixed solution;
[0065] Step 2: adding oxalic acid to the mixed solution prepared in step 1, stirring and heating to 90° C., reacting for 12 hours to obtain a reaction solution, wherein the mass ratio of methyltrimethoxysilane, phenolic resin and oxalic acid is 1:1.2:0.01;
[0066] Step 3: heating the reaction solution obtained in step 2 to 135° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0067] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0068] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 160℃ for 5h;
[0069] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1200°C, the heating rate is 0.6°C / min, and the temperature is kept for 60 minutes after the heating is completed to obtain a carbon material;
[0070] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2400° C. and a graphitization time of 60 min to obtain a graphitized material;
[0071] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2200° C., and the porous carbon material is obtained after the purification process is completed.
[0072] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0073] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0074] Unit fracture toughness = fracture toughness / density;
[0075] The calculated unit fracture toughness of the porous carbon material is 21.7 (MPa•m 1 / 2 *cm 3 ) / g.
[0076] The SEM image of the porous carbon material prepared in this embodiment is as follows: Figure 1 shown.
[0077] Comparative Example 1
[0078] This comparative example provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0079] Step 1: Mixing phenolic resin and carbon fiber of equal weight in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0080] Step 2: Place the mixture obtained in step 1 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 160℃ for 5h;
[0081] Step 3: isolating oxygen in a carbonization furnace for carbonization at a temperature of 1200°C and a heating rate of 0.6°C / min. After the heating is completed, the carbonization is kept for 60 minutes to obtain a carbon material;
[0082] Step 4: placing the carbon material obtained in step 3 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2400° C. and a graphitization time of 60 min to obtain a graphitized material;
[0083] Step 5: placing the graphitized material obtained in step 4 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2200° C., and the porous carbon material is obtained after the purification process is completed.
[0084] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0085] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0086] Unit fracture toughness = fracture toughness / density;
[0087] The calculated unit fracture toughness of the porous carbon material is 11.3 (MPa•m 1 / 2 *cm 3 ) / g.
[0088] Comparative Example 2
[0089] This comparative example provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0090] Step 1: Mix vinyl trimethoxysilane and phenolic resin, and stir and mix them evenly at 70° C. to obtain a mixed solution;
[0091] Step 2: adding oxalic acid to the mixed solution prepared in step 1, stirring and heating to 90° C., reacting for 12 hours to obtain a reaction solution, wherein the mass ratio of vinyl trimethoxysilane, phenolic resin and oxalic acid is 1:1.2:0.01;
[0092] Step 3: heating the reaction solution obtained in step 2 to 135° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0093] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0094] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 160℃ for 5h;
[0095] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1200°C, the heating rate is 0.6°C / min, and the temperature is kept for 60 minutes after the heating is completed to obtain a carbon material;
[0096] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2400° C. and a graphitization time of 60 min to obtain a graphitized material;
[0097] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2200° C., and the porous carbon material is obtained after the purification process is completed.
[0098] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0099] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0100] Unit fracture toughness = fracture toughness / density;
[0101] The calculated unit fracture toughness of the porous carbon material is 17.3 (MPa•m 1 / 2 *cm 3 ) / g.
[0102] Comparative Example 3
[0103] This comparative example provides a porous carbon fiber material with high fracture toughness and a preparation method thereof, comprising the following steps:
[0104] Step 1: Mix the silica particles with the phenolic resin, and stir and mix them evenly at 70° C. to obtain a mixed solution;
[0105] Step 2: adding oxalic acid to the mixed solution prepared in step 1, stirring and heating to 90° C., reacting for 12 hours to obtain a reaction solution, wherein the mass ratio of the silica particles, the phenolic resin and the oxalic acid is 1:1.2:0.01;
[0106] Step 3: heating the reaction solution obtained in step 2 to 135° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin;
[0107] Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture, wherein the average length of the carbon fiber is 200 microns and the average diameter is 14 microns;
[0108] Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 160℃ for 5h;
[0109] Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1200°C, the heating rate is 0.6°C / min, and the temperature is kept for 60 minutes after the heating is completed to obtain a carbon material;
[0110] Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2400° C. and a graphitization time of 60 min to obtain a graphitized material;
[0111] Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2200° C., and the porous carbon material is obtained after the purification process is completed.
[0112] The density of the porous carbon material was measured to be 0.92 g / cm 3 .
[0113] The fracture toughness of the porous carbon material is measured by the test method described in the single edge pre-cracked beam (SEPB) method of GB / T 23806-2009 fine ceramic fracture toughness test method, and then according to the formula:
[0114] Unit fracture toughness = fracture toughness / density;
[0115] The calculated unit fracture toughness of the porous carbon material is 12.7 (MPa•m 1 / 2 *cm 3 ) / g.
Claims
1. A porous carbon fiber material with high fracture toughness, characterized in that: The unit fracture toughness of the porous carbon fiber material is 16-22 (MPa•m 1 / 2 *cm 3 ) / g; Among them, unit fracture toughness = fracture toughness / density; Density: 0.92g / cm 3 ; The test standard for fracture toughness is GB / T 23806-2009; The porous carbon fiber material is prepared by the following method: Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 60-80° C. to obtain a mixed solution; Step 2: Add oxalic acid to the mixed solution prepared in step 1, stir and heat to 80-100° C., react for 10-14 hours to obtain a reaction solution; Step 3: heating the reaction solution obtained in step 2 to 130-140° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin; Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture; Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 150-170℃ for 4-6h; Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1100-1300°C, the heating rate is 0.4-1°C / min, and the temperature is kept for 30-90 minutes after the heating is completed to obtain a carbon material; Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2300-2500° C. and a graphitization time of 30-90 min to obtain a graphitized material; Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2000-2400° C., and the porous carbon material is obtained after the purification process is completed; The mass ratio of the methyltrimethoxysilane, the phenolic resin and the oxalic acid is 1:1-1.5:0.005-0.
02.
2. A porous carbon fiber material with high fracture toughness as claimed in claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 16-17 (MPa•m 1 / 2 *cm 3 ) / g.
3. A porous carbon fiber material with high fracture toughness as claimed in claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 17-18 (MPa•m 1 / 2 *cm 3 ) / g.
4. A porous carbon fiber material with high fracture toughness as claimed in claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 18-19 (MPa•m 1 / 2 *cm 3 ) / g.
5. The porous carbon fiber material with high fracture toughness according to claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 19-20 (MPa•m 1 / 2 *cm 3 ) / g.
6. The porous carbon fiber material with high fracture toughness according to claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 20-21 (MPa•m 1 / 2 *cm 3 ) / g.
7. The porous carbon fiber material with high fracture toughness according to claim 1, characterized in that: The unit fracture toughness of the porous carbon fiber material is 21-22 (MPa•m 1 / 2 *cm 3 ) / g.
8. A method for preparing a porous carbon fiber material with high fracture toughness as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Mix methyltrimethoxysilane and phenolic resin, and stir and mix them evenly at 60-80° C. to obtain a mixed solution; Step 2: Add oxalic acid to the mixed solution prepared in step 1, stir and heat to 80-100° C., react for 10-14 hours to obtain a reaction solution; Step 3: heating the reaction solution obtained in step 2 to 130-140° C., distilling under reduced pressure, and collecting the remaining solid matter after distillation to obtain a silicon-modified phenolic resin; Step 4: Mixing the silicon-modified phenolic resin prepared in step 3 with carbon fiber of equal mass in a mixer until the mixture is uniform to obtain a mixture; Step 5: Place the mixture obtained in step 4 in a cold pressing mold and press it into a blank with a density of 0.93 g / cm 3 , and heat and cure at 150-170℃ for 4-6h; Step 6: isolating oxygen in the carbonization furnace for carbonization, the carbonization temperature is 1100-1300°C, the heating rate is 0.4-1°C / min, and the temperature is kept for 30-90 minutes after the heating is completed to obtain a carbon material; Step 7: placing the carbon material obtained in step 6 into a graphitization furnace, graphitizing under argon protection, with a graphitization temperature of 2300-2500° C. and a graphitization time of 30-90 min to obtain a graphitized material; Step 8: placing the graphitized material obtained in step 7 in a purification furnace for purification, the purification gas is chlorine, the purification temperature is 2000-2400° C., and the porous carbon material is obtained after the purification process is completed.
9. The method for preparing a porous carbon fiber material with high fracture toughness according to claim 8, characterized in that: The average length of the carbon fibers is 200 micrometers, and the average diameter is 14 micrometers.
10. The method for preparing a porous carbon fiber material with high fracture toughness according to claim 8, characterized in that: The mass ratio of the methyltrimethoxysilane, the phenolic resin and the oxalic acid is 1:1-1.5:0.005-0.02.