Water-resistant wood-plastic laminate floor and manufacturing method thereof

By controlling the preparation of silica microspheres and titanium-silicon composite microspheres, combined with high-temperature boiling treatment of wood powder, the problems of water absorption and mechanical properties of wood plastic composite materials are solved, and the water resistance and mechanical properties are improved, forming a Excellent waterproofing and adhesion.

CN118206790BActive Publication Date: 2024-11-22VOHRINGER HOME TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410042294.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-11-22
Estimated Expiration
2044-01-11

AI Technical Summary

Technical Problem

The existing wood-plastic composite materials have problems such as volume deformation, reduced mechanical properties, and mold after water absorption, resulting in insufficient water resistance and urgently need to be improved.

Method used

By controlling the preparation process of silica microspheres, nanosilica particles are formed to coat polystyrene microspheres, titanium-silicon composite microspheres and silicone-modified castor oil are introduced, combining the polyamino structure and sealing in the polyurethane emulsion. The end silane coupling agent forms a micro-nano structure to improve the waterproof performance of the coating; at the same time, the wood powder is boiled at high temperature to increase the pore size distribution and surface area, and improve the binding force between the wood powder and the composite resin.

Benefits of technology

The water resistance and mechanical properties of wood-plastic composite materials are significantly improved, and the primary and secondary waterproof structures are formed, which enhances the adhesion and stability of the coating after curing, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of wood-plastic composite materials, and discloses a water-resistant wood-plastic reinforced composite floor and a manufacturing method thereof. Wood powder is boiled in boiling water for 3-4 hours, filtered, and dried to obtain dry wood powder; polypropylene, butyl acrylate, methyl methacrylate, maleic anhydride, and dicumyl peroxide are mixed evenly, extruded into granules, and dried to obtain a compatibilizer; the dry wood powder and polypropylene are mixed evenly, the compatibilizer is added and mixed evenly, extruded into granules, and injection molded to obtain a wood-plastic floor blank; a composite resin emulsion and a photoinitiator are ultrasonically mixed evenly, the wood-plastic floor blank is impregnated therein, taken out and dried at room temperature, vacuum dried, and ultraviolet light cured to obtain a water-resistant wood-plastic reinforced composite floor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wood-plastic composite materials, in particular to a water-resistant wood-plastic reinforced composite floor and a manufacturing method thereof. Background Art

[0002] The wood-plastic composite process is one of the important modification technologies that converts monomers into polymers to fill the wood cell cavity and improve the physical and mechanical properties of wood. The wood-plastic composite material prepared by it has better water resistance than ordinary wood. However, with the continuous improvement of living standards, people are increasingly concerned about the water resistance of wood-plastic composite materials, especially the high water absorption rate, volume deformation after water absorption, reduced mechanical properties, and mold. Solving these technical problems is urgent.

[0003] Therefore, it is of great significance to invent a water-resistant wood-plastic laminate floor and a method for making the same. Summary of the invention

[0004] The object of the present invention is to provide a water-resistant wood-plastic laminate floor and a manufacturing method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for making a water-resistant wood-plastic laminate floor comprises the following steps:

[0007] S1: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C in an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and kept warm for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane and titanium silicon composite microspheres are added and cooled to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and kept warm for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and kept warm for reaction for 1-1.5 hours, and deionized water is added for emulsification for 30-45 minutes to obtain a composite resin emulsion;

[0008] S2: Boil wood powder in boiling water for 3-4 hours, filter, and dry to obtain dry wood powder; mix polypropylene, butyl acrylate, methyl methacrylate, maleic anhydride, and diisopropylbenzene peroxide evenly, extrude and granulate, and dry to obtain a compatibilizer; mix dry wood powder and polypropylene evenly, add the compatibilizer and mix evenly, extrude and granulate, and injection mold to obtain a wood-plastic flooring blank; ultrasonically mix the composite resin emulsion and the photoinitiator at 30-35°C, immerse the wood-plastic flooring blank therein, take out and dry at room temperature for 7 days, vacuum dry at 60-65°C for 1 day, and UV-curing to obtain a water-resistant wood-plastic laminate composite floor.

[0009] Furthermore, the preparation method of the titanium-silicon composite microspheres comprises the following steps:

[0010] The silica microspheres are placed at 600-605° C. and calcined for 3-3.5 hours to obtain hollow silica microspheres; the hollow silica microspheres are ultrasonically dispersed in toluene, isopropoxy tris(ethylenediamino-N-ethoxy) titanate is added, ultrasonically dispersed, heated to 70-80° C. for reaction for 3-5 hours, centrifuged, allowed to stand and precipitate in tert-butanol, filtered, and vacuum dried to obtain titanium-silicon composite microspheres.

[0011] Furthermore, the mass ratio of hollow silica microspheres to isopropoxy tris(ethylenediamino-N-ethoxy) titanate is 1:(4-5).

[0012] Furthermore, the method for preparing silica microspheres comprises the following steps:

[0013] Add styrene to polyvinyl pyrrolidone solution and stir evenly, add potassium persulfate aqueous solution, heat to reflux reaction for 12-14 hours, wash, and dry to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir to react for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres.

[0014] Furthermore, the mass ratio of styrene: potassium persulfate in the potassium persulfate aqueous solution is 12:(0.36-0.48); the mass ratio of polystyrene microspheres: tetraethyl orthosilicate is 2:(4-5); and the concentration of the ammonia water is 2-3wt%.

[0015] Furthermore, the method for preparing silicone-modified castor oil comprises the following steps:

[0016] Castor oil, mercaptopropyl trimethoxysilane and benzoin dimethyl ether are reacted under argon atmosphere and irradiated with ultraviolet light for 12-24 hours to obtain siloxane-modified castor oil.

[0017] Furthermore, the mass ratio of castor oil:mercaptopropyltrimethoxysilane is (1.57-1.62):1; the amount of benzoin dimethyl ether added is 3-3.5wt% of the total mass of castor oil and mercaptopropyltrimethoxysilane.

[0018] Furthermore, the proportion of each component in the composite resin emulsion, by mass percentage, isophorone diisocyanate 8-10%, siloxane-modified castor oil 2.5-10%, castor oil 9-14%, 1,4-butanediol 0.7-0.8%, 2,2-dihydroxymethylpropionic acid 1.6-1.7%, trimethylolpropane 0.5-0.6%, titanium silicon composite microspheres 3-5%, mercaptopropyl trimethoxysilane 0.4-0.5%, hydroxyethyl acrylate 0.3-0.7%, dimethylaminoethyl methacrylate 2.3-2.6%, and the rest is deionized water.

[0019] Furthermore, the proportions of the components in the compatibilizer, by mass, are 100-120 parts of polypropylene, 10-12 parts of butyl acrylate, 10-12 parts of methyl methacrylate, 10-12 parts of maleic anhydride, and 0.3-0.5 parts of dicumyl peroxide; the mass ratio of dry wood powder: polypropylene: compatibilizer is 100:100:(5-10); and the amount of photoinitiator added is 3-4wt% of the mass of the composite resin emulsion.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] The invention controls the particle size of nano silicon dioxide coated on the surface of a polystyrene microsphere template by controlling the use of ammonia catalyst and tetraethyl orthosilicate in a reaction system during the preparation of silicon dioxide microspheres; the produced nano silicon dioxide particles can completely coat the polystyrene template to form complete "mulberry-shaped" microspheres; further, polyvinyl pyrrolidone is used as a stabilizing dispersant and a connecting agent, and through the adsorption effect of polyvinyl pyrrolidone, on the one hand, the polystyrene microspheres can be adsorbed or grafted on the surface of the polystyrene microspheres to improve the dispersibility and stability of the polystyrene microspheres; on the other hand, tetraethyl orthosilicate can be adsorbed on the surface of the polystyrene microspheres, so that the nano silicon dioxide particles hydrolyzed and condensed under the action of ammonia are coated on the surface of the polystyrene microspheres to serve as a connecting agent between the polystyrene microspheres and the nano silicon dioxide pieces, and finally the silicon dioxide microspheres containing microstructures are prepared.

[0022] In order to improve the dispersibility of silica microspheres in polyurethane emulsion, isopropoxy tri(ethylenediamine-N-ethoxy) titanate was grafted on its surface, and titanium-silicon composite microspheres with a multi-amino structure were introduced on the surface of silica microspheres. The titanium-silicon composite microspheres were successfully introduced into the polyurethane emulsion as a chain extender. On the one hand, the dispersibility problem of titanium-silicon composite microspheres in polyurethane emulsion was solved. On the other hand, when the polyurethane emulsion formed a coating on the surface of the wood-plastic composite material, the granular protrusion structure generated after the introduction of the titanium-silicon composite microspheres was evenly distributed on the coating surface, forming a primary waterproof structure. Since the titanium-silicon composite microspheres are coated with nano-silicon dioxide particles, the surface has finer nanoparticles, forming a secondary waterproof structure. At the same time, under the connection of the polyurethane end-capped silane coupling agent, these titanium-silicon composite microspheres will also be connected to each other to form a network structure, and finally form a micro-nano structure on the coating surface. The gaps between these structures can capture air molecules between the solid-liquid interface when in contact with water, forming a Cassie-state composite surface, which greatly improves the water resistance of the wood-plastic composite template after the coating is cured.

[0023] The present invention boils wood powder in water at high temperature to expand the cellulose in the wood powder and cause some cellulose microfibrils to slip, thereby widening the pore size distribution of the wood powder and increasing the specific surface area. This can not only improve the interfacial compatibility of the wood powder and polypropylene under the action of the compatibilizer, but also improve the reaction of the hydroxyl groups on the surface of the wood powder with the active functional groups (siloxane) in the composite resin emulsion, thereby improving the bonding force between the coating and the wood-plastic composite wood board.

[0024] The invention uses mercaptopropyl trimethoxysilane to graft and modify castor oil, introduces silane into polyol, introduces soft segments with silane side chains into polyurethane structures, and further improves the water resistance of the coating under the synergistic effect of further end-capping of mercaptopropyl trimethoxysilane; in order to further improve the adhesion of the coating after emulsion curing and ensure the stability of the emulsion, an acrylate structure is introduced into polyurethane, and a hydrophilic group is introduced into a molecular chain segment, thereby ensuring the stability of the composite resin emulsion and giving the composite resin emulsion the ability of ultraviolet light curing; a wood-plastic composite template impregnated with the composite resin emulsion is dried at room temperature and then placed in an oven for drying for primary curing, and then secondary cured by an ultraviolet light curing machine, thereby greatly enhancing the bonding force between the coating and the wood-plastic composite wood board and giving the wood-plastic composite wood board excellent water resistance and mechanical properties. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following examples, castor oil was purchased from Aladdin Reagent Co., Ltd.; polyvinyl pyrrolidone was purchased from Sinopharm Chemical Reagent Co., Ltd.; polypropylene was purchased from Sinopec Guangzhou Branch, with a melt flow rate of 8 to 15 g / 10 min and a model of CJS-700; wood powder was purchased from Jiangmen Weihua Spice Factory, with a specification of eucalyptus powder, 80 mesh; and the remaining raw materials were commercially available.

[0027] Example 1: A method for preparing a water-resistant wood-plastic laminate floor: S1: 15.7 g of castor oil, 10 g of mercaptopropyl trimethoxysilane, and 0.771 g of benzoin dimethyl ether were reacted under an argon atmosphere under ultraviolet light for 18 hours to obtain siloxane-modified castor oil;

[0028] S2: Add styrene to polyvinyl pyrrolidone solution and stir evenly, add potassium persulfate aqueous solution, heat to reflux reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir to react for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0029] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:4; the concentration of ammonia water is 2wt%;

[0030] S3: calcining the silica microspheres at 600°C for 3 hours to obtain hollow silica microspheres; ultrasonically dispersing the hollow silica microspheres in toluene, adding isopropoxy tris(ethylenediamino-N-ethoxy) titanate, ultrasonically dispersing, heating to 70°C for 3 hours, centrifuging for 30 minutes, dispersing the solids in tert-butanol for 10 minutes of ultrasonic oscillation, centrifuging for 30 minutes, repeating the above centrifugation-oscillation-centrifugation operation 3 times, placing the solids after centrifugation in tert-butanol for static precipitation for 24 hours, filtering, and vacuum drying at 70°C for 2 hours to obtain titanium-silicon composite microspheres;

[0031] The mass ratio of hollow silica microspheres to isopropoxy tris(ethylenediamine-N-ethoxy) titanate is 1:4;

[0032] S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and kept warm for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and cooled to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and kept warm for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and kept warm for reaction for 1-1.5 hours, deionized water is added for emulsification for 30-45 minutes, and acetone is removed at 60°C to obtain a composite resin emulsion;

[0033] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 2.5%, castor oil 14%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 3%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.7%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0034] S5: Boil wood powder in boiling water for 3 hours, filter, and dry to obtain dry wood powder; mix polypropylene, butyl acrylate, methyl methacrylate, maleic anhydride, and diisopropylbenzene peroxide evenly, extrude and granulate, and dry to obtain a compatibilizer; mix dry wood powder and polypropylene evenly, add the compatibilizer and mix evenly, extrude and granulate, and injection mold to obtain a wood-plastic flooring blank; ultrasonically mix the composite resin emulsion and the photoinitiator at 30°C, immerse the wood-plastic flooring blank therein, take out and dry at room temperature for 7 days, vacuum dry at 60°C for 1 day, and UV-curing to obtain a water-resistant wood-plastic laminate composite floor;

[0035] Among them, 100 parts of polypropylene, 10 parts of butyl acrylate, 10 parts of methyl methacrylate, 10 parts of maleic anhydride, 0.3 parts of dicumyl peroxide; the mass ratio of dry wood powder: polypropylene: compatibilizer is 100:100:5; the amount of photoinitiator added is 3wt% of the mass of the composite resin emulsion.

[0036] Embodiment 2: A method for preparing a water-resistant wood-plastic laminate floor: S2: Add styrene to a polyvinyl pyrrolidone solution and stir evenly, add a potassium persulfate aqueous solution, heat to reflux for reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in an ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir for reaction for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0037] Wherein, the mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:5; the concentration of the ammonia water is 2wt%;

[0038] The remaining steps are the same as those in Example 1.

[0039] Example 3: A method for preparing a water-resistant wood-plastic laminate floor: S2: Add styrene to a polyvinyl pyrrolidone solution and stir evenly, add a potassium persulfate aqueous solution, heat to reflux for reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, and dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in an ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir for reaction for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0040] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:4; the concentration of ammonia water is 3wt%;

[0041] The remaining steps are the same as those in Example 1.

[0042] Example 4: A method for preparing a water-resistant wood-plastic laminate floor: S2: Add styrene to a polyvinyl pyrrolidone solution and stir evenly, add a potassium persulfate aqueous solution, heat to reflux for reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, and dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in an ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir for reaction for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0043] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:5; the concentration of ammonia water is 3wt%;

[0044] The remaining steps are the same as those in Example 1.

[0045] Embodiment 5: A method for making a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept to react until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C to react until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and the temperature is heated to 40-45°C to react until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and the temperature is kept to react until the -NCO group reacts completely, dimethylaminoethyl methacrylate is added and the temperature is kept to react for 1-1.5 hours, deionized water is added and emulsified for 30-45 minutes, and acetone is removed at 60°C to obtain a composite resin emulsion;

[0046] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 5%, castor oil 12%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 3%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.3%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0047] The remaining steps are the same as those in Example 4.

[0048] Embodiment 6: A method for making a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 min; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept constant for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and the temperature is heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and the temperature is kept constant for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and the temperature is kept constant for reaction for 1-1.5 h, deionized water is added for emulsification for 30-45 min, and acetone is removed at 60°C to obtain a composite resin emulsion;

[0049] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 10%, castor oil 9%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 3%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.7%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0050] The remaining steps are the same as those in Example 4.

[0051] Embodiment 7: A method for preparing a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 min; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept to react until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C to react until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and the temperature is heated to 40-45°C to react until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and the temperature is kept to react until the -NCO group reacts completely, dimethylaminoethyl methacrylate is added and the temperature is kept to react for 1-1.5 h, deionized water is added and emulsified for 30-45 min, and acetone is removed at 60°C to obtain a composite resin emulsion;

[0052] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 10%, castor oil 9%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 4%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.5%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0053] The remaining steps are the same as those in Example 4.

[0054] Example 8: A method for making a water-resistant wood-plastic laminate floor: S4: Heat isophorone diisocyanate, siloxane-modified castor oil, and castor oil to 75-80°C in an argon atmosphere and react for 30-60 minutes; add 1,4-butanediol and 2,2-dihydroxymethylpropionic acid and keep warm to react until the -NCO group content reaches a predetermined value; add trimethylolpropane, titanium silicon composite microspheres, and acetone and cool to 30-35°C to react until the -NCO group content is stable; add mercaptopropyltrimethoxysilane and heat to 40-45°C to react until the -NCO group content reaches a predetermined value; add hydroxyethyl acrylate and keep warm to react until the -NCO group reacts completely, add dimethylaminoethyl methacrylate and keep warm to react for 1-1.5 hours, add deionized water for emulsification for 30-45 minutes, heat to 60°C to remove acetone, and obtain a composite resin emulsion;

[0055] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 10%, castor oil 9%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 5%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.3%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0056] The remaining steps are the same as those in Example 4.

[0057] Comparative Example 1: A method for preparing a water-resistant wood-plastic laminate floor: S2: Add styrene to a polyvinyl pyrrolidone solution and stir evenly, add a potassium persulfate aqueous solution, heat to reflux for reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, and dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in an ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir for reaction for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0058] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:6; the concentration of ammonia water is 2wt%;

[0059] The remaining steps are the same as those in Example 1.

[0060] Comparative Example 2: A method for preparing a water-resistant wood-plastic laminate floor: S2: Add styrene to a polyvinyl pyrrolidone solution and stir evenly, add a potassium persulfate aqueous solution, heat to reflux for reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, and dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in an ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir for reaction for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0061] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:4; the concentration of ammonia water is 5wt%;

[0062] The remaining steps are the same as those in Example 1.

[0063] Comparative Example 3: A method for preparing a water-resistant wood-plastic laminate floor: S1: 15.7 g of castor oil, 10 g of mercaptopropyl trimethoxysilane, and 0.771 g of benzoin dimethyl ether were reacted under an argon atmosphere under ultraviolet light for 18 hours to obtain siloxane-modified castor oil;

[0064] S2: Add styrene to polyvinyl pyrrolidone solution and stir evenly, add potassium persulfate aqueous solution, heat to reflux reaction for 12 hours, wash with ethanol and deionized water alternately for 3 times, dry at 60°C for 1 day to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32°C, stir to react for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres;

[0065] The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:0.3; the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:4; the concentration of ammonia water is 2wt%;

[0066] S3: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and kept warm for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane is added, the temperature is lowered to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyltrimethoxysilane is added and heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and kept warm for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and kept warm for reaction for 1-1.5 hours, deionized water is added, emulsified for 30-45 minutes, silica microspheres are added and stirred evenly to obtain a composite resin emulsion;

[0067] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 2.5%, castor oil 14%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 5%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.7%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0068] S4: Boil wood powder in boiling water for 3 hours, filter, and dry to obtain dry wood powder; mix polypropylene, butyl acrylate, methyl methacrylate, maleic anhydride, and diisopropylbenzene peroxide evenly, extrude and granulate, and dry to obtain a compatibilizer; mix dry wood powder and polypropylene evenly, add the compatibilizer and mix evenly, extrude and granulate, and injection mold to obtain a wood-plastic flooring blank; ultrasonically mix the composite resin emulsion and the photoinitiator at 30°C, immerse the wood-plastic flooring blank therein, take out and dry at room temperature for 7 days, vacuum dry at 60°C for 1 day, and UV-curing to obtain a water-resistant wood-plastic laminate composite floor;

[0069] Among them, 100 parts of polypropylene, 10 parts of butyl acrylate, 10 parts of methyl methacrylate, 10 parts of maleic anhydride, 0.3 parts of dicumyl peroxide; the mass ratio of dry wood powder: polypropylene: compatibilizer is 100:100:5; the amount of photoinitiator added is 3wt% of the mass of the composite resin emulsion;

[0070] The remaining steps are the same as those in Example 1.

[0071] Comparative Example 4: A method for preparing a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept constant for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and the temperature is heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and the temperature is kept constant for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and the temperature is kept constant for reaction for 1-1.5 hours, deionized water is added for emulsification for 30-45 minutes, and the acetone is removed at 60°C to obtain a composite resin emulsion;

[0072] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 15%, castor oil 9%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 3%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.7%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0073] The remaining steps are the same as those in Example 1.

[0074] Comparative Example 5: A method for preparing a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept constant for reaction until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C for reaction until the -NCO group content is stable; mercaptopropyl trimethoxysilane is added and the temperature is heated to 40-45°C for reaction until the -NCO group content reaches a predetermined value; hydroxyethyl acrylate is added and the temperature is kept constant for reaction until the -NCO group reaction is complete, dimethylaminoethyl methacrylate is added and the temperature is kept constant for reaction for 1-1.5 hours, deionized water is added and emulsified for 30-45 minutes, and the acetone is removed at 60°C to obtain a composite resin emulsion;

[0075] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 2.5%, castor oil 14%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium silicon composite microspheres 7%, mercaptopropyl trimethoxysilane 0.4%, hydroxyethyl acrylate 0.7%, dimethylaminoethyl methacrylate 2.3%, and the rest is deionized water;

[0076] The remaining steps are the same as those in Example 1.

[0077] Comparative Example 6: A method for preparing a water-resistant wood-plastic laminate floor: S4: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and the temperature is kept to react until the -NCO group content reaches a predetermined value; trimethylolpropane, titanium silicon composite microspheres, and acetone are added and the temperature is lowered to 30-35°C to react until the -NCO group content is stable; mercaptopropyltrimethoxysilane is added and heated to 40-45°C to react until the -NCO group reacts completely, triethylamine is added and the temperature is kept to react for 1-1.5 hours, deionized water is added for emulsification for 30-45 minutes, and the acetone is removed at 60°C to obtain a composite resin emulsion;

[0078] Among them, isophorone diisocyanate 8%, siloxane-modified castor oil 2.5%, castor oil 14%, 1,4-butanediol 0.7%, 2,2-dihydroxymethylpropionic acid 1.6%, trimethylolpropane 0.5%, titanium-silicon composite microspheres 3%, mercaptopropyl trimethoxysilane 0.4%, triethylamine 2.3%, and the rest is deionized water;

[0079] The remaining steps are the same as those in Example 1.

[0080] Test: Water contact angle test: water drops were added to the surface of the water-resistant wood-plastic laminate composite floor, and the contact angle was tested by a surface contact angle meter; the test objects were the water-resistant wood-plastic laminate composite floors prepared in Examples 1-8 and Comparative Examples 1-3.

[0081] Water absorption test: The water-resistant wood-plastic laminated composite flooring dried to constant weight was immersed in water for one week, and the mass change before and after immersion was recorded to calculate the water absorption rate W; the test objects were the water-resistant wood-plastic laminated composite floors prepared in Examples 1-8 and Comparative Examples 1-3.

[0082] W(%)=(m1-m0) / m0×100%;

[0083] Among them, m1 is the weight after water absorption; m0 is the constant weight after drying.

[0084] Stability test: After the emulsion is centrifuged in a centrifuge at a speed of 3000 r / min for 15 minutes, if there is no stratification or precipitation, it is considered to have a stable storage period of at least 6 months; test object: emulsions prepared in Examples 1-8 and Comparative Examples 4-6.

[0085] Table 1 Water resistance test data of wood-plastic composite wood board

[0086] Contact angle / ° Water absorption rate W / % Example 1 141.7 3.43 Example 2 144.8 3.35 Example 3 144.6 3.37 Example 4 147.8 3.08 Example 5 150.2 2.82 Example 6 151.4 2.72 Example 7 153.6 2.49 Example 8 156.5 2.25 Comparative Example 1 131.8 4.56 Comparative Example 2 133.2 4.44 Comparative Example 3 120.3 5.67

[0087] Table 2 Composite resin emulsion stability test data

[0088] Emulsion centrifugal stability Example 1 Stablize Example 2 Stablize Example 3 Stablize Example 4 Stablize Example 5 Stablize Example 6 Stablize Example 7 Stablize Example 8 Stablize Comparative Example 4 Slightly delaminated Comparative Example 5 Slightly delaminated Comparative Example 6 Layering

[0089] Conclusion: The wood-plastic composite wood board prepared in this application has excellent water resistance.

[0090] In Comparative Example 1, due to excessive addition of ethyl orthosilicate during the preparation of silica nanospheres, the generated silica particles are too large and easily fall off the surface of the polystyrene microspheres, and a complete "mulberry-shaped" microsphere cannot be formed, resulting in reduced water resistance;

[0091] In comparative example 2, due to excessive addition of ammonia catalyst during the preparation of silica nanospheres, the hydrolysis reaction was too fast, resulting in the generated silica particles being too large in size, and easily falling off the surface of the polystyrene microspheres, and failing to form complete "mulberry-shaped" microspheres; resulting in reduced water resistance;

[0092] In Comparative Example 3, the composite resin emulsion is prepared by directly blending the silicon dioxide nanoparticles with the polyurethane emulsion, which results in reduced water resistance.

[0093] In Comparative Examples 4 and 5, too much siloxane-modified castor oil and titanium-silicon composite microspheres were added, and there were too many hydrophobic group ions, resulting in reduced emulsion stability;

[0094] In Comparative Example 6, no acrylate group was introduced, resulting in reduced emulsion stability.

[0095] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for producing a water-resistant wood-plastic laminate floor. Features: The following steps are involved: S1: isophorone diisocyanate, siloxane-modified castor oil, and castor oil are heated to 75-80°C under an argon atmosphere for reaction for 30-60 minutes; 1,4-butanediol and 2,2-dihydroxymethylpropionic acid are added and kept warm for reaction; trimethylolpropane and titanium silicon composite microspheres are added and cooled to 30-35°C for reaction; mercaptopropyl trimethoxysilane is added and heated to 40-45°C for reaction; hydroxyethyl acrylate is added and kept warm for reaction until the -NCO group reacts completely, dimethylaminoethyl methacrylate is added and kept warm for reaction for 1-1.5 hours, and deionized water is added and emulsified for 30-45 minutes to obtain a composite resin emulsion; S2: Boil wood powder in boiling water for 3-4 hours, filter, and dry to obtain dry wood powder; mix polypropylene, butyl acrylate, methyl methacrylate, maleic anhydride, and dicumyl peroxide evenly, extrude and granulate, and dry to obtain a compatibilizer; mix dry wood powder and polypropylene evenly, add the compatibilizer and mix evenly, extrude and granulate, and injection mold to obtain a WPC flooring blank; ultrasonically mix the composite resin emulsion and the photoinitiator at 30-35°C, and immerse the WPC flooring blank therein. After being taken out and dried at room temperature, the floor is vacuum dried at 60-65°C and cured by ultraviolet light to obtain a water-resistant wood-plastic laminate floor; The preparation method of the titanium-silicon composite microspheres comprises the following steps: The silica microspheres are placed at 600-605° C. and calcined for 3-3.5 hours to obtain hollow silica microspheres; the hollow silica microspheres are ultrasonically dispersed in toluene, isopropoxy tris(ethylenediamino-N-ethoxy) titanate is added, ultrasonically dispersed, heated to 70-80° C. for reaction for 3-5 hours, centrifuged, allowed to stand and precipitate in tert-butanol, filtered, and vacuum dried to obtain titanium-silicon composite microspheres; The method for preparing silicone-modified castor oil comprises the following steps: Castor oil, mercaptopropyl trimethoxysilane and benzoin dimethyl ether are reacted under argon atmosphere and irradiated with ultraviolet light for 12-24 hours to obtain siloxane-modified castor oil; The proportions of the components in the composite resin emulsion, by mass percentage, are 8-10% of isophorone diisocyanate, 2.5-10% of siloxane-modified castor oil, 9-14% of castor oil, 0.7-0.8% of 1,4-butanediol, 1.6-1.7% of 2,2-dihydroxymethylpropionic acid, 0.5-0.6% of trimethylolpropane, 3-5% of titanium-silicon composite microspheres, 0.4-0.5% of mercaptopropyl trimethoxysilane, 0.3-0.7% of hydroxyethyl acrylate, 2.3-2.6% of dimethylaminoethyl methacrylate, and the rest is deionized water; The mass ratio of hollow silica microspheres to isopropoxy tris(ethylenediamino-N-ethoxy) titanate is 1:(4-5); The method for preparing silica microspheres comprises the following steps: Add styrene to polyvinyl pyrrolidone solution and stir evenly, add potassium persulfate aqueous solution, heat to reflux reaction for 12-14 hours, wash, and dry to obtain polystyrene microspheres; ultrasonically disperse the polystyrene microspheres in ethanol solution, add ammonia water, stir evenly, add tetraethyl orthosilicate, heat to 30-32° C., stir to react for 12-14 hours, centrifuge, wash, and dry to obtain silica microspheres; The mass ratio of styrene to potassium persulfate in the potassium persulfate aqueous solution is 12:(0.36-0.48); the mass ratio of polystyrene microspheres to tetraethyl orthosilicate is 2:(4-5); the concentration of the ammonia water is 2-3wt%; The mass ratio of castor oil to mercaptopropyl trimethoxysilane is (1.57-1.62):1; the amount of benzoin dimethyl ether added is 3-3.5wt% of the total mass of castor oil and mercaptopropyl trimethoxysilane; The proportions of the components in the compatibilizer, by mass, are 100-120 parts of polypropylene, 10-12 parts of butyl acrylate, 10-12 parts of methyl methacrylate, 10-12 parts of maleic anhydride, and 0.3-0.5 parts of dicumyl peroxide; the mass ratio of dry wood powder: polypropylene: compatibilizer is 100:100:(5-10); the amount of photoinitiator added is 3-4wt% of the mass of the composite resin emulsion.

2. The water-resistant wood-plastic laminate flooring prepared by the method for preparing the water-resistant wood-plastic laminate flooring according to claim 1.