A highly flame-retardant PET base film and preparation method thereof
By introducing silicon phosphorus flame retardants and metallized fillers into the PET base film, the problem of insufficient flame retardancy and bonding performance of the PET base film is solved, and a PET base film with high flame retardancy and UV aging resistance is prepared, which is suitable for in the fields of composite current collectors and batteries.
Patent Information
- Application Number
- CN202410411333.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The flame retardant performance of the PET base film is poor, and the bonding performance with the metal layer is insufficient, which affects the overall performance of the composite current collector.
Chlorinated spirocyclic phosphates were synthesized using phosphorus oxychloride and pentaerythritol, and combined with 4-propenyloxy-2-hydroxybenzophenone and 2,4-divinyl-2,4,6,6,8,8 -The reaction of hexamethylcyclotetrasiloxane generates a silicon-phosphorus flame retardant, which is combined with carbon fiber, copper-coated carbon fiber and silver-coated polystyrene microspheres to prepare a highly flame-retardant PET base through extrusion casting and biaxial stretching processes membrane.
It significantly improves the flame retardant performance and UV aging resistance of the PET base film, and at the same time enhances the bonding performance between the base film and the metal layer, making it suitable for composite current collectors and batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PET films, in particular to a highly flame-retardant PET base film and a preparation method thereof. Background Art
[0002] The current collector is one of the indispensable components of lithium-ion batteries. The positive and negative electrodes of lithium-ion batteries are equipped with different current collector materials. The positive electrode is aluminum foil and the negative electrode is copper foil. Due to the limitations of traditional current collectors, composite current collectors have gradually become our preferred solution. Composite current collectors use some organic matter to replace metals and are designed to be similar to a "sandwich" structure. The middle layer is a polymer film, and metal layers are plated on both sides of the polymer film. Polymer films are generally made of PET, PP, PI and other materials. Due to the rapid development of composite current collectors, the performance requirements for polymer films are also getting higher and higher.
[0003] PET base film is one of the most commonly used base films on the market, but its flame retardant performance is poor. In addition, as the middle layer, how to ensure the bonding performance between the PET base film and the metal layers on both sides is an urgent concern of existing R&D personnel and a technical problem that we urgently need to solve. Summary of the invention
[0004] The object of the present invention is to provide a highly flame-retardant PET base film and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a highly flame-retardant PET base film comprises the following steps:
[0007] Step 1: Mix phosphorus oxychloride and pentaerythritol, heat to 80-85°C under nitrogen atmosphere, react for 0.5-1h, continue to heat to 110-115°C, continue to react for 6-7h, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate;
[0008] Maintaining a nitrogen atmosphere, the chlorinated spirocyclic phosphate and formic acid were mixed, stirred at 30-40° C. for 0.5-1 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature was raised to 60-65° C., 4-propyleneoxy-2-hydroxybenzophenone was added, and the temperature was kept for reaction for 1-2 h, and 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 24-28 h. The product was collected by centrifugation to obtain a flame retardant;
[0009] Step 2: mixing the carbon fiber, the copper-coated carbon fiber and the silver-coated polystyrene microspheres to obtain a composite filler;
[0010] The PET resin, silane coupling agent, compound filler, antioxidant, lubricant and flame retardant are mixed, extruded and cast into a film, and biaxially stretched to obtain a PET base film.
[0011] In a more optimized solution, in step 2, the amount of each component is: by mass, 100 parts of PET resin, 4-6 parts of silane coupling agent, 6-8 parts of compound filler, 1-1.5 parts of antioxidant, 0.3-0.5 parts of lubricant, and 5-10 parts of flame retardant.
[0012] In a more optimized solution, in step 2, the mass ratio of the carbon fiber, the copper-plated carbon fiber and the silver-plated polystyrene microspheres is 2:3:1; the antioxidant is antioxidant 168, and the lubricant is ethylene bisstearamide.
[0013] In a more optimized scheme, in step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:(4.5-5.5); the molar ratio of the chlorinated spirocyclic phosphate to formic acid is 1:(2-2.2); the molar ratio of the chlorinated spirocyclic phosphate, 4-propyleneoxy-2-hydroxybenzophenone, and 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane is (1.5-2):1:1.
[0014] A more optimized solution is that in step 2, the extrusion temperature is 275~285℃, the transverse stretching ratio is 3~5 during biaxial stretching, the longitudinal stretching ratio is 2~4, the stretching temperature is 105~110℃, the stretching rate is 110mm / s, and the heat setting temperature is 220~230℃.
[0015] A more optimized solution is to prepare copper-plated carbon fiber as follows: take carbon fiber, place it in a heating furnace and burn it for 50~60 minutes at a temperature of 480~500℃, then soak it in an acetone solution for 50~60 minutes, wash and dry it, and after drying, place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber.
[0016] A more optimized solution is that the electroplating solution components are: copper sulfate 40-50 g / L, sodium tartrate 10-12 g / L, sodium citrate 85-90 g / L, sodium nitrate 12-13 g / L, and the balance is deionized water; the pH of the electroplating solution is 9-10, and the process parameters of copper electroplating are: electroplating temperature is 40-45 ° C, time is 30-40 min, current density is 1-2 A / dm 2 .
[0017] A more optimized solution is to prepare silver-coated polystyrene microspheres as follows:
[0018] Dissolve polyvinyl pyrrolidone in ethanol, stir for 30-40 minutes under nitrogen atmosphere at 70-75°C, then add styrene and azobisisobutyronitrile, keep warm at 70-75°C for 10-11 hours, wash and dry to obtain polystyrene microspheres;
[0019] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, and ultrasonic dispersion was performed for 10 to 20 minutes. After being taken out, they were sensitized by stannous chloride solution and activated by palladium chloride solution. Then, they were transferred to silver ammonia solution, stirred at 30 to 35°C for 3 to 5 minutes, formaldehyde solution was added, stirring was continued for 20 to 30 minutes, filtered, washed, and vacuum dried to obtain silver-coated polystyrene microspheres.
[0020] In a more optimized solution, the amount of polyvinyl pyrrolidone is 3-4wt% of styrene; the amount of azobisisobutyronitrile is 1-1.5wt% of styrene; the concentration of potassium dichromate is 0.1-0.2mol / L, the concentration of sodium dodecylbenzenesulfonate is 0.01-0.02mol / L, and the concentration of concentrated sulfuric acid is 60-65mL / L; the concentration of stannous chloride is 0.1-0.2mol / L, the concentration of palladium chloride is 0.2-0.3g / L, the amount of formaldehyde solution is 10-12mL / L, the amount of ammonia water in the silver ammonia solution is 60-65mL / L, and the mass ratio of the amount of silver nitrate in the silver ammonia solution to the styrene microspheres is 1:(2-2.5).
[0021] A more optimized solution is a highly flame-retardant PET base film prepared according to any of the preparation methods described above.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] The invention discloses a highly flame-retardant PET base film and a preparation method thereof. The method comprises mixing materials such as PET resin, silane coupling agent, compound filler, antioxidant and flame retardant, extruding and casting to form a film, and stretching the film through a biaxial stretching process, wherein the transverse stretching ratio during biaxial stretching is 3-5, the longitudinal stretching ratio is 2-4, the stretching temperature is 105-110° C., and the stretching rate is 110 mm / s. The finally prepared PET base film has high comprehensive mechanical properties, excellent flame retardancy, and improved UV aging resistance.
[0024] In this scheme, the present application first uses phosphorus oxychloride and pentaerythritol as raw materials to generate chlorinated spirocyclic phosphate, and uses chlorinated spirocyclic phosphate, 4-propyleneoxy-2-hydroxybenzophenone and 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane for grafting, and the C=C in the system reacts with PH to obtain a silicon-phosphorus flame retardant. The addition of the silicon-phosphorus flame retardant can effectively improve the flame retardant properties of the PET base film, and the introduction of 4-propyleneoxy-2-hydroxybenzophenone can improve the anti-ultraviolet aging performance of the PET base film. In addition, in order to avoid the introduction of the flame retardant affecting the tensile strength of the base film, the scheme uses 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane as a raw material to ensure the flame retardant properties of the product while ensuring its tensile strength.
[0025] At the same time, the scheme also adds compound fillers, which are compounded with carbon fibers, copper-plated carbon fibers and silver-plated polystyrene microspheres. On the one hand, the introduction of compound fillers can effectively improve the tensile strength of the base film. On the other hand, the scheme performs surface metallization treatment on some fillers, electroplating copper on the surface of carbon fibers to form copper-plated carbon fibers, and using polystyrene microspheres as cores, electroplating silver on the surface to generate silver-plated polystyrene microspheres. Carbon fibers, copper-plated carbon fibers and silver-plated polystyrene microspheres are compounded as conductive fillers. The introduction of metallized fillers in the base film can effectively improve the surface bonding performance between the base film and the metal, and the bonding performance is even better in the subsequent preparation of composite current collectors.
[0026] The present application discloses a method for preparing a highly flame-retardant PET base film. Through this method, a PET base film with excellent mechanical properties is prepared. The PET base film has high flame retardancy and improved resistance to ultraviolet aging. It can be widely used in the processing of composite current collectors or batteries and has high practicality. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In this embodiment, the silane coupling agent is KH-550, the antioxidant is antioxidant 168, and the lubricant is ethylene bis stearamide. The length of the carbon fiber is 1-2 mm and the diameter is 3 μm; the PET resin is PETCZ-333.
[0029] Embodiment 1: A method for preparing a highly flame-retardant PET base film, comprising the following steps:
[0030] Step 1: Mix 0.5 mol of phosphorus oxychloride and 0.1 mol of pentaerythritol, heat to 80°C under nitrogen atmosphere, react for 1 hour, continue to heat to 110°C, continue to react for 7 hours, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate.
[0031] Maintaining a nitrogen atmosphere, 0.2 mol of chlorinated spirocyclic phosphate and 0.4 mol of formic acid were mixed, stirred at 30°C for 1 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature was raised to 60°C, 0.1 mol of 4-propyleneoxy-2-hydroxybenzophenone was added, and the reaction was kept warm for 2 h, and then 0.1 mol of 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 24 h. The product was collected by centrifugation to obtain a flame retardant.
[0032] Step 2: Mix the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres to obtain a composite filler; the mass ratio of the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres is 2:3:1.
[0033] In parts by mass, 100 parts of PET resin, 5 parts of silane coupling agent, 6 parts of compound filler, 1.5 parts of antioxidant, 0.5 parts of lubricant and 8 parts of flame retardant are mixed, extruded and cast into film, the extrusion temperature is 275°C, and biaxial stretching is performed. During biaxial stretching, the transverse stretching ratio is 3, the longitudinal stretching ratio is 4, the stretching temperature is 110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220°C to obtain a PET base film.
[0034] The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 60 minutes at a temperature of 480°C, then place it in an acetone solution and soak it for 50 minutes, wash it with water and dry it, and then place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber. The electroplating solution components are: 45g / L copper sulfate, 12g / L sodium tartrate, 85g / L sodium citrate, 12g / L sodium nitrate, and the balance is deionized water; the process parameters of copper electroplating are: electroplating temperature of 45°C, time of 30min, current density of 2A / dm 2 .
[0035] The preparation steps of silver-coated polystyrene microspheres are as follows: 1.26 g of polyvinyl pyrrolidone is dissolved in 100 mL of ethanol, stirred for 30 min under a nitrogen atmosphere at 75°C, 36 g of styrene and 0.54 g of azobisisobutyronitrile are added, the mixture is reacted at 70°C for 11 h, washed and dried to obtain polystyrene microspheres.
[0036] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, ultrasonically dispersed for 10 minutes, taken out, sensitized by stannous chloride solution, activated by palladium chloride solution, and then transferred to silver ammonia solution, stirred at 30°C for 5 minutes, added formaldehyde solution, continued to stir for 30 minutes, filtered and washed, and vacuum dried to obtain silver-plated polystyrene microspheres. The concentration of potassium dichromate was 0.1 mol / L, the concentration of sodium dodecylbenzene sulfonate was 0.01 mol / L, and the concentration of concentrated sulfuric acid was 60 mL / L; the concentration of stannous chloride was 0.1 mol / L, the concentration of palladium chloride was 0.2 g / L, the amount of formaldehyde solution was 10 mL / L, the amount of ammonia water in the silver ammonia solution was 60 mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to the styrene microspheres was 1:2.
[0037] Embodiment 2: A method for preparing a highly flame-retardant PET base film, comprising the following steps:
[0038] Step 1: Mix 0.5 mol of phosphorus oxychloride and 0.1 mol of pentaerythritol, heat to 85°C under nitrogen atmosphere, react for 1 hour, continue to heat to 115°C, continue to react for 6.5 hours, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate.
[0039] Maintaining a nitrogen atmosphere, 0.2 mol of chlorinated spirocyclic phosphate and 0.4 mol of formic acid were mixed, stirred at 35°C for 1 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature was raised to 65°C, 0.1 mol of 4-propyleneoxy-2-hydroxybenzophenone was added, and the reaction was kept warm for 1.5 h. Then 0.1 mol of 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 26 h. The product was collected by centrifugation to obtain a flame retardant.
[0040] Step 2: Mix the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres to obtain a composite filler; the mass ratio of the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres is 2:3:1.
[0041] In parts by mass, 100 parts of PET resin, 5 parts of silane coupling agent, 7 parts of compound filler, 1.5 parts of antioxidant, 0.5 parts of lubricant and 9 parts of flame retardant are mixed, extruded and cast into a film, the extrusion temperature is 275°C, and biaxial stretching is performed. During biaxial stretching, the transverse stretching ratio is 3, the longitudinal stretching ratio is 4, the stretching temperature is 110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220°C to obtain a PET base film.
[0042] The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 60 minutes at a temperature of 480°C, then place it in an acetone solution and soak it for 55 minutes, wash it with water and dry it, and then place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber. The electroplating solution components are: 45g / L copper sulfate, 12g / L sodium tartrate, 85g / L sodium citrate, 12g / L sodium nitrate, and the balance is deionized water; the process parameters of copper electroplating are: electroplating temperature is 45°C, time is 30min, current density is 2A / dm 2 .
[0043] The preparation steps of silver-coated polystyrene microspheres are as follows: 1.26 g of polyvinyl pyrrolidone is dissolved in 100 mL of ethanol, stirred for 35 min under a nitrogen atmosphere at 75°C, 36 g of styrene and 0.54 g of azobisisobutyronitrile are added, the mixture is kept warm at 75°C for 10 h, washed and dried to obtain polystyrene microspheres.
[0044] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, ultrasonically dispersed for 15 minutes, taken out, sensitized by stannous chloride solution, activated by palladium chloride solution, and then transferred to silver ammonia solution, stirred at 35°C for 4 minutes, added formaldehyde solution, continued to stir for 30 minutes, filtered and washed, and vacuum dried to obtain silver-plated polystyrene microspheres. The concentration of potassium dichromate was 0.1 mol / L, the concentration of sodium dodecylbenzene sulfonate was 0.01 mol / L, and the concentration of concentrated sulfuric acid was 60 mL / L; the concentration of stannous chloride was 0.1 mol / L, the concentration of palladium chloride was 0.2 g / L, the amount of formaldehyde solution was 10 mL / L, the amount of ammonia water in the silver ammonia solution was 60 mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to the styrene microspheres was 1:2.
[0045] Embodiment 3: A method for preparing a highly flame-retardant PET base film, comprising the following steps:
[0046] Step 1: Mix 0.5 mol of phosphorus oxychloride and 0.1 mol of pentaerythritol, heat to 85°C under nitrogen atmosphere, react for 0.5 h, continue to heat to 115°C, continue to react for 6 h, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate.
[0047] Maintaining a nitrogen atmosphere, 0.2 mol of chlorinated spirocyclic phosphate and 0.4 mol of formic acid were mixed, stirred at 40°C for 0.5 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature was raised to 65°C, 0.1 mol of 4-propyleneoxy-2-hydroxybenzophenone was added, and the reaction was kept warm for 1 h, and then 0.1 mol of 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 28 h. The product was collected by centrifugation to obtain a flame retardant.
[0048] Step 2: Mix the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres to obtain a composite filler; the mass ratio of the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres is 2:3:1.
[0049] In parts by mass, 100 parts of PET resin, 5 parts of silane coupling agent, 7 parts of compound filler, 1.5 parts of antioxidant, 0.5 parts of lubricant and 10 parts of flame retardant are mixed, extruded and cast into a film, the extrusion temperature is 275°C, and biaxial stretching is performed. During biaxial stretching, the transverse stretching ratio is 3, the longitudinal stretching ratio is 4, the stretching temperature is 110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220°C to obtain a PET base film.
[0050] The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 60 minutes at a temperature of 480°C, then place it in an acetone solution and soak it for 60 minutes, wash it with water and dry it, and then place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber. The electroplating solution components are: 45g / L copper sulfate, 12g / L sodium tartrate, 85g / L sodium citrate, 12g / L sodium nitrate, and the balance is deionized water; the process parameters of copper electroplating are: electroplating temperature is 45°C, time is 30min, current density is 2A / dm 2 .
[0051] The preparation steps of silver-coated polystyrene microspheres are as follows: 1.26 g of polyvinyl pyrrolidone is dissolved in 100 mL of ethanol, stirred for 40 min under a nitrogen atmosphere at 75°C, 36 g of styrene and 0.54 g of azobisisobutyronitrile are added, the mixture is reacted at 75°C for 10 h, washed and dried to obtain polystyrene microspheres.
[0052] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, ultrasonically dispersed for 20 minutes, taken out, sensitized by stannous chloride solution, activated by palladium chloride solution, and then transferred to silver ammonia solution, stirred at 35°C for 5 minutes, added formaldehyde solution, continued to stir for 30 minutes, filtered and washed, and vacuum dried to obtain silver-plated polystyrene microspheres. The concentration of potassium dichromate was 0.1 mol / L, the concentration of sodium dodecylbenzene sulfonate was 0.01 mol / L, and the concentration of concentrated sulfuric acid was 60 mL / L; the concentration of stannous chloride was 0.1 mol / L, the concentration of palladium chloride was 0.2 g / L, the amount of formaldehyde solution was 10 mL / L, the amount of ammonia water in the silver ammonia solution was 60 mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to the styrene microspheres was 1:2.
[0053] Comparative Example 1: Taking Example 3 as the control group, the amount of the flame retardant in Comparative Example 1 was adjusted to 15 parts, and the other steps remained unchanged.
[0054] A method for preparing a highly flame-retardant PET base film comprises the following steps:
[0055] Step 1: Mix 0.5 mol of phosphorus oxychloride and 0.1 mol of pentaerythritol, heat to 85°C under nitrogen atmosphere, react for 0.5 h, continue to heat to 115°C, continue to react for 6 h, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate.
[0056] Maintaining a nitrogen atmosphere, 0.2 mol of chlorinated spirocyclic phosphate and 0.4 mol of formic acid were mixed, stirred at 40°C for 0.5 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature was raised to 65°C, 0.1 mol of 4-propyleneoxy-2-hydroxybenzophenone was added, and the reaction was kept warm for 1 h, and then 0.1 mol of 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 28 h. The product was collected by centrifugation to obtain a flame retardant.
[0057] Step 2: Mix the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres to obtain a composite filler; the mass ratio of the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres is 2:3:1.
[0058] In parts by mass, 100 parts of PET resin, 5 parts of silane coupling agent, 7 parts of compound filler, 1.5 parts of antioxidant, 0.5 parts of lubricant and 15 parts of flame retardant are mixed, extruded and cast into a film, the extrusion temperature is 275°C, and biaxial stretching is performed. During biaxial stretching, the transverse stretching ratio is 3, the longitudinal stretching ratio is 4, the stretching temperature is 110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220°C to obtain a PET base film.
[0059] The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 60 minutes at a temperature of 480°C, then place it in an acetone solution and soak it for 60 minutes, wash it with water and dry it, and then place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber. The electroplating solution components are: 45g / L copper sulfate, 12g / L sodium tartrate, 85g / L sodium citrate, 12g / L sodium nitrate, and the balance is deionized water; the process parameters of copper electroplating are: electroplating temperature is 45°C, time is 30min, current density is 2A / dm 2 .
[0060] The preparation steps of silver-coated polystyrene microspheres are as follows: 1.26 g of polyvinyl pyrrolidone is dissolved in 100 mL of ethanol, stirred for 40 min under a nitrogen atmosphere at 75°C, 36 g of styrene and 0.54 g of azobisisobutyronitrile are added, the mixture is reacted at 75°C for 10 h, washed and dried to obtain polystyrene microspheres.
[0061] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, ultrasonically dispersed for 20 minutes, taken out, sensitized by stannous chloride solution, activated by palladium chloride solution, and then transferred to silver ammonia solution, stirred at 35°C for 5 minutes, added formaldehyde solution, continued to stir for 30 minutes, filtered and washed, and vacuum dried to obtain silver-plated polystyrene microspheres. The concentration of potassium dichromate was 0.1 mol / L, the concentration of sodium dodecylbenzene sulfonate was 0.01 mol / L, and the concentration of concentrated sulfuric acid was 60 mL / L; the concentration of stannous chloride was 0.1 mol / L, the concentration of palladium chloride was 0.2 g / L, the amount of formaldehyde solution was 10 mL / L, the amount of ammonia water in the silver ammonia solution was 60 mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to the styrene microspheres was 1:2.
[0062] Comparative Example 2: Taking Example 3 as the control group, the preparation process of the flame retardant in Comparative Example 2 was adjusted, and the other steps remained unchanged.
[0063] A method for preparing a highly flame-retardant PET base film comprises the following steps:
[0064] Step 1: Mix 0.5 mol of phosphorus oxychloride and 0.1 mol of pentaerythritol, heat to 85°C under nitrogen atmosphere, react for 0.5 h, continue to heat to 115°C, continue to react for 6 h, cool after the reaction, collect the product, and vacuum dry to obtain chlorinated spirocyclic phosphate.
[0065] Maintaining a nitrogen atmosphere, 0.2 mol of chlorinated spirocyclic phosphate and 0.4 mol of formic acid were mixed, stirred at 40°C for 0.5 h, the product was collected, washed and dried, and then dissolved in N,N-dimethylformamide. The temperature was raised to 65°C, and the reaction was kept warm for 1 h. Then 0.1 mol of 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane was added, and the reaction was continued for 28 h. The product was collected by centrifugation to obtain a flame retardant.
[0066] Step 2: Mix the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres to obtain a composite filler; the mass ratio of the carbon fiber, copper-plated carbon fiber and silver-plated polystyrene microspheres is 2:3:1.
[0067] In parts by mass, 100 parts of PET resin, 5 parts of silane coupling agent, 7 parts of compound filler, 1.5 parts of antioxidant, 0.5 parts of lubricant and 10 parts of flame retardant are mixed, extruded and cast into a film, the extrusion temperature is 275°C, and biaxial stretching is performed. During biaxial stretching, the transverse stretching ratio is 3, the longitudinal stretching ratio is 4, the stretching temperature is 110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220°C to obtain a PET base film.
[0068] The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 60 minutes at a temperature of 480°C, then place it in an acetone solution and soak it for 60 minutes, wash it with water and dry it, and then place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber. The electroplating solution components are: 45g / L copper sulfate, 12g / L sodium tartrate, 85g / L sodium citrate, 12g / L sodium nitrate, and the balance is deionized water; the process parameters of copper electroplating are: electroplating temperature is 45°C, time is 30min, current density is 2A / dm 2 .
[0069] The preparation steps of silver-coated polystyrene microspheres are as follows: 1.26 g of polyvinyl pyrrolidone is dissolved in 100 mL of ethanol, stirred for 40 min under a nitrogen atmosphere at 75°C, 36 g of styrene and 0.54 g of azobisisobutyronitrile are added, the mixture is reacted at 75°C for 10 h, washed and dried to obtain polystyrene microspheres.
[0070] Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid were mixed, polystyrene microspheres were added, ultrasonically dispersed for 20 minutes, taken out, sensitized by stannous chloride solution, activated by palladium chloride solution, and then transferred to silver ammonia solution, stirred at 35°C for 5 minutes, added formaldehyde solution, continued to stir for 30 minutes, filtered and washed, and vacuum dried to obtain silver-plated polystyrene microspheres. The concentration of potassium dichromate was 0.1 mol / L, the concentration of sodium dodecylbenzene sulfonate was 0.01 mol / L, and the concentration of concentrated sulfuric acid was 60 mL / L; the concentration of stannous chloride was 0.1 mol / L, the concentration of palladium chloride was 0.2 g / L, the amount of formaldehyde solution was 10 mL / L, the amount of ammonia water in the silver ammonia solution was 60 mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to the styrene microspheres was 1:2.
[0071] Detection experiment:
[0072] The PET base film (thickness of 3 μm) prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was tested for tensile strength according to the method disclosed in GB / T1040.1. The width of the sample was 15 mm, the length was 200 mm, and the tensile rate during the test was 100 mm / min. The limiting oxygen index of the PET base film was tested according to the method disclosed in GB / T2046. The PET base film was irradiated in a UV aging box with a total irradiation energy of 60 kWh / m 2 The light source is UVB (280~320nm), and the irradiance of the lamp is 180W / m 2 , retest the tensile strength after UV aging and record the retention rate.
[0073]
[0074] Conclusion: This application discloses a method for preparing a highly flame-retardant PET base film. Through this scheme, a PET base film with excellent mechanical properties is prepared. The PET base film has high flame retardancy and improved resistance to ultraviolet aging. It can be widely used in the processing of composite current collectors or batteries and has high practicality.
[0075] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a highly flame-retardant PET base film, Features: The following steps are involved: Step 1: phosphorus oxychloride and pentaerythritol are mixed, heated to 80-85° C. under a nitrogen atmosphere, reacted for 0.5-1 h, and then heated to 110-115° C., and reacted for 6-7 h. After the reaction is completed, the mixture is cooled, the product is collected, and vacuum dried to obtain chlorinated spirocyclic phosphate; Maintaining a nitrogen atmosphere, the chlorinated spirocyclic phosphate and formic acid are mixed, stirred at 30-40° C. for 0.5-1 h, the product is collected, washed and dried, and then dissolved in N,N-dimethylformamide, the temperature is raised to 60-65° C., 4-propyleneoxy-2-hydroxybenzophenone is added, the temperature is kept to react for 1-2 h, 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane is added, the reaction is continued for 24-28 h, and the product is collected by centrifugation to obtain a flame retardant; Step 2: mixing the carbon fiber, the copper-coated carbon fiber and the silver-coated polystyrene microspheres to obtain a composite filler; The PET resin, silane coupling agent, compound filler, antioxidant, lubricant and flame retardant are mixed, extruded and cast into a film, and biaxially stretched to obtain a PET base film; In step 2, the amount of each component is: by mass, 100 parts of PET resin, 4-6 parts of silane coupling agent, 6-8 parts of compound filler, 1-1.5 parts of antioxidant, 0.3-0.5 parts of lubricant, and 5-10 parts of flame retardant.
2. A method for preparing a highly flame-retardant PET base film according to claim 1, Features: In step 2, the mass ratio of the carbon fiber, the copper-plated carbon fiber and the silver-plated polystyrene microspheres is 2:3:1; the antioxidant is antioxidant 168, and the lubricant is ethylene bisstearamide.
3. The method for preparing a highly flame-retardant PET base film according to claim 1, Features: In step 1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:(4.5-5.5); the molar ratio of the chlorinated spirocyclic phosphate and formic acid is 1:(2-2.2); the molar ratio of the chlorinated spirocyclic phosphate, 4-propyleneoxy-2-hydroxybenzophenone, and 2,4-divinyl-2,4,6,6,8,8-hexamethylcyclotetrasiloxane is (1.5-2):1:
1.
4. The method for preparing a highly flame-retardant PET base film according to claim 1, Features: In step 2, the extrusion temperature is 275-285°C, the transverse stretching ratio is 3-5 during biaxial stretching, the longitudinal stretching ratio is 2-4, the stretching temperature is 105-110°C, the stretching rate is 110 mm / s, and the heat setting temperature is 220-230°C.
5. The method for preparing a highly flame-retardant PET base film according to claim 1, Features: The preparation steps of copper-plated carbon fiber are as follows: take carbon fiber, place it in a heating furnace and burn it for 50 to 60 minutes at a temperature of 480 to 500°C, then soak it in an acetone solution for 50 to 60 minutes, wash and dry it, and after drying, place it in an electroplating solution to electroplate copper on the surface to obtain copper-plated carbon fiber.
6. A method for preparing a highly flame-retardant PET base film according to claim 5, Features: The electroplating solution comprises: 40-50 g / L copper sulfate, 10-12 g / L sodium tartrate, 85-90 g / L sodium citrate, 12-13 g / L sodium nitrate, and the balance is deionized water; the pH of the electroplating solution is 9-10, and the process parameters of copper electroplating are: electroplating temperature is 40-45° C., time is 30-40 min, current density is 1-2 A / dm 2 .
7. The method for preparing a highly flame-retardant PET base film according to claim 1, Features: The preparation steps of silver-coated polystyrene microspheres are as follows: Dissolve polyvinyl pyrrolidone in ethanol, stir for 30-40 minutes under nitrogen atmosphere at 70-75°C, then add styrene and azobisisobutyronitrile, keep warm at 70-75°C for 10-11 hours, wash and dry to obtain polystyrene microspheres; Potassium dichromate, sodium dodecylbenzene sulfonate and concentrated sulfuric acid are mixed, polystyrene microspheres are added, and ultrasonic dispersion is carried out for 10 to 20 minutes. After being taken out, they are sensitized by stannous chloride solution and activated by palladium chloride solution. Then, they are transferred to silver ammonia solution, stirred at 30 to 35°C for 3 to 5 minutes, formaldehyde solution is added, stirring is continued for 20 to 30 minutes, filtered, washed, and vacuum dried to obtain silver-coated polystyrene microspheres.
8. The method for preparing a highly flame-retardant PET base film according to claim 7, Features: The amount of polyvinyl pyrrolidone is 3-4wt% of styrene; the amount of azobisisobutyronitrile is 1-1.5wt% of styrene; the concentration of stannous chloride is 0.1-0.2mol / L, the concentration of palladium chloride is 0.2-0.3g / L, the amount of formaldehyde solution is 10-12mL / L, the amount of ammonia water in the silver ammonia solution is 60-65mL / L, and the mass ratio of silver nitrate in the silver ammonia solution to styrene microspheres is 1: (2~2.5)。 9. A highly flame-retardant PET base film prepared according to the preparation method according to any one of claims 1 to 8.