A high thermal conductivity rubber composite material and preparation method thereof

By using modified two-dimensional flake thermally conductive fillers and granular thermally conductive flame-retardant fillers in thermally conductive rubber composite materials, a continuous thermal conductive network and uniform dispersion are formed, which solves the problem of insufficient performance of existing materials and achieves high thermal conductivity and flame retardancy. And the improvement of mechanical properties is suitable for fields such as high-power electronic components and new energy vehicles.

CN118222015BActive Publication Date: 2024-10-29XIAMEN LIANBO RUBBER PROD CO LTD

Patent Information

Application Number
CN202410286337.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-10-29
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Existing thermally conductive rubber composite materials have poor performance in thermal conductivity, flame retardancy and insulation, and are difficult to meet the heat dissipation needs of high-power electronic components and new energy vehicles.

Method used

It uses natural rubber and styrene-butadiene rubber as the matrix, combined with two-dimensional flaky thermally conductive fillers (composed of flaky boron nitride, graphite flakes and alumina) and granular thermally conductive flame-retardant fillers (composed of aluminum nitride and magnesium hydroxide). , through vinyltrimethoxysilane and plasma modification, a continuous three-dimensional thermally conductive filler network is formed and uniformly dispersed to improve thermal conductivity and flame retardant properties, and coupling agents, activators, antioxidants and accelerators are added to enhance mechanical properties and compatibility.

Benefits of technology

The thermal conductivity, flame retardancy and mechanical properties are significantly improved, which meets the heat dissipation needs of high-power products. At the same time, the preparation process is simplified, the production cycle is shortened, and the material is environmentally friendly and meets environmental requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004739261080000101
    Figure BDA0004739261080000101
  • Figure BDA0004739261080000111
    Figure BDA0004739261080000111
Patent Text Reader

Abstract

The present application relates to the technical field of thermally conductive elastic materials, and in particular to a high thermally conductive rubber composite material and a preparation method thereof. A high thermally conductive rubber composite material, by mass, includes the following raw materials: 45-50 parts of natural rubber, 45-50 parts of styrene-butadiene rubber, 10-12 parts of plasticizer, 2-3 parts of coupling agent, 30-35 parts of two-dimensional sheet-like thermally conductive filler, 30-35 parts of granular thermally conductive flame-retardant filler, 5-8 parts of activator, 2-4 parts of stearic acid, 1-1.5 parts of antioxidant, 1-1.5 parts of accelerator, and 1-2 parts of vulcanizing agent. The high thermally conductive rubber composite material of the present application has excellent mechanical properties, good thermal conductivity, good flame retardancy, good insulation, and adopts a simple preparation process, has a fast vulcanization speed, and also meets the requirements of energy saving and environmental protection. It can meet the thermal conductivity and heat dissipation needs of high thermally conductive rubber composite materials in the fields of consumer electronics, new energy vehicles, LED lighting, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thermally conductive elastic materials, and in particular to a high thermally conductive rubber composite material and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology, electronic components tend to be integrated, miniaturized and high-power. In order to solve the heat conduction and heat dissipation problems of high-power products such as electronic chips, new energy vehicle power batteries, high-power stage lights, LED lighting, etc., various thermally conductive elastic materials (such as thermally conductive gaskets, thermally conductive gels, etc.) have been widely used. However, the thermal conductivity, flame retardancy, insulation and other properties of existing thermally conductive rubber composite materials are poor and need to be further improved.

[0003] Therefore, it is of great significance to develop a rubber composite material with good thermal conductivity, flame retardancy and insulation. Summary of the invention

[0004] The purpose of this application is to provide a high thermal conductivity rubber composite material and a preparation method thereof in view of the deficiencies of the current technology.

[0005] In a first aspect, the present application provides a high thermal conductivity rubber composite material, which adopts the following technical solution:

[0006] A high thermal conductivity rubber composite material, comprising the following raw materials by weight: 45-50 parts of natural rubber, 45-50 parts of styrene-butadiene rubber, 10-12 parts of plasticizer, 2-3 parts of coupling agent, 30-35 parts of two-dimensional sheet-like thermal conductive filler, 30-35 parts of granular thermal conductive flame retardant filler, 5-8 parts of activator, 2-4 parts of stearic acid, 1-1.5 parts of antioxidant, 1-1.5 parts of accelerator, 1-2 parts of vulcanizer, wherein the two-dimensional sheet-like thermal conductive filler is The thermal filler is composed of flaky boron nitride, flaky graphite and flaky aluminum oxide in a mass ratio of 8:3:1-3, and is modified by vinyltrimethoxysilane and then plasma modified; the granular thermal conductive flame retardant filler is composed of aluminum nitride and magnesium hydroxide in a mass ratio of 1:5, and is modified by vinyltrimethoxysilane and then plasma modified; the mass fraction ratio of the two-dimensional flaky thermal conductive filler and the granular thermal conductive flame retardant filler is 1:1.

[0007] By adopting the above technical scheme, natural rubber and styrene butadiene rubber: natural rubber and styrene butadiene rubber are the main components of the rubber matrix, which give the material good elasticity, toughness and softness, and improve the processability and durability of the composite material. Plasticizer: Plasticizer can increase the plasticity and softness of rubber materials, making the material easier to process and form. Coupling agent: Coupling agent can enhance the adhesion between different components, make different components better combined with each other, and improve the mechanical properties and durability of the material. Two-dimensional flake thermal conductive filler: Two-dimensional flake thermal conductive fillers composed of flake boron nitride, flake graphite flakes and flake aluminum oxide form a continuous three-dimensional thermal conductive filler network in the rubber matrix resin. They have high thermal conductivity, play a role in heat conduction in the material, and improve the thermal conductivity. Granular thermal conductive flame retardant filler: Granular thermal conductive flame retardant fillers composed of aluminum nitride and magnesium hydroxide are uniformly dispersed in the rubber matrix resin. They have good flame retardant properties, can effectively prevent the spread of flames, and improve the flame retardant properties of the material. Surfactant: The surfactant promotes the cross-linking reaction between the vulcanizing agent and the rubber molecules by regulating the vulcanization reaction of the rubber material, thereby improving the mechanical properties and durability of the material. Stearic acid: Stearic acid acts as a lubricant in the material, improving the processing performance of the material, making the material easier to process and form. Anti-aging agent: Anti-aging agent has antioxidant properties, which can effectively resist material aging and extend the service life of the material. Accelerator: Accelerator can accelerate the vulcanization reaction, increase the vulcanization speed of the material, and shorten the production cycle. Vulcanizing agent: Vulcanizing agent is the main component in rubber material, which is used for the cross-linking reaction of rubber to improve the durability and strength of the material. In short, the high thermal conductivity rubber composite material of the present application improves the thermal conductivity, flame retardant properties and mechanical properties through the synergistic effect of different raw materials, and meets the needs of thermal conduction and heat dissipation. At the same time, the vinyltrimethoxysilane modification and plasma modification in the modification process improve the compatibility and dispersibility of the material.

[0008] Preferably, the two-dimensional flaky thermally conductive filler has an average radial dimension of 10-20 μm and an average thickness of 80-200 nm; and the average particle size of the granular thermally conductive flame-retardant filler is 1-10 μm.

[0009] Preferably, the method for preparing the two-dimensional sheet-shaped thermally conductive filler comprises the following steps:

[0010] S31, according to the weight ratio, 1.5 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed and stirred to obtain a mixture A;

[0011] S32, adding 80 parts of flaky boron nitride, 30 parts of flaky graphite sheets and 10-30 parts of flaky aluminum oxide to mixture A according to their weight percentages; then heating to 42° C. and stirring at a speed of 300 r / min for 120 min to obtain a silanized two-dimensional flaky thermal conductive filler mixed liquid;

[0012] S33. Filter the silanized two-dimensional flaky thermally conductive filler mixture, wash with ethanol, dry and grind at 75°C, and then perform plasma surface modification for 20 seconds at a power of 2KW and an oxygen volume concentration of 10% to obtain a two-dimensional flaky thermally conductive filler, wherein the two-dimensional flaky thermally conductive filler has an average radial size of 10-20μm and an average thickness of 80-200nm.

[0013] By adopting the above technical scheme, flake boron nitride: has a high thermal conductivity and can improve the thermal conductivity of the composite material. Flake graphite: graphite has a high thermal conductivity and can improve the thermal conductivity of the composite material. Flake aluminum oxide: aluminum oxide has a high thermal conductivity and can improve the thermal conductivity of the composite material. Through vinyl trimethoxysilane modification treatment, the compatibility and dispersibility of the two-dimensional flake thermal conductive filler with the rubber matrix resin can be improved, so that it can be better combined with the rubber matrix. Through the action of plasma, the surface properties of the two-dimensional flake thermal conductive filler are improved, and the interaction with the rubber matrix is ​​increased. While improving the thermal conductivity, the dispersion and use performance of the material are further improved. In summary, the preparation method of the two-dimensional flake thermal conductive filler enables it to form a continuous three-dimensional thermal conductive filler network in the rubber matrix resin, which increases the thermal conductivity. Through vinyl trimethoxysilane modification and plasma modification, its compatibility and dispersibility with the rubber matrix are improved, and the thermal conductivity and use performance are further improved.

[0014] Preferably, the method for preparing the granular thermally conductive flame retardant filler comprises the following steps:

[0015] S41, according to the mass parts, 2 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed, and stirred to obtain a mixture B;

[0016] S42, adding 100 parts of aluminum nitride and 100 parts of magnesium hydroxide to mixture B according to their mass fractions; then heating to 45° C. and stirring at a speed of 200 r / min for 150 min to obtain a silanized granular thermally conductive flame-retardant filler mixed liquid;

[0017] S43. Filter the silanized granular thermally conductive flame-retardant filler mixture, wash with ethanol, dry at 75°C, grind, and then perform plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a granular thermally conductive flame-retardant filler with an average particle size of 1-10 μm.

[0018] By adopting the above technical scheme, aluminum nitride: has high thermal conductivity and high temperature resistance, and can improve the thermal conductivity of the composite material. Magnesium hydroxide: has flame retardant properties, and can improve the flame retardant properties of the composite material. Through vinyl trimethoxysilane modification treatment, the compatibility and dispersibility of the granular thermal conductive flame retardant filler with the rubber matrix resin can be improved, so that it can be better combined with the rubber matrix. Through the action of plasma, the surface properties of the granular thermal conductive flame retardant filler are improved, and the interaction with the rubber matrix is ​​increased. While improving the thermal conductivity and flame retardant properties, the dispersibility and use performance of the material are further improved. In summary, the preparation method of the granular thermal conductive flame retardant filler makes it uniformly dispersed in the silicone rubber matrix resin, and the two-dimensional flaky thermal conductive filler forms a continuous three-dimensional thermal conductive filler network, which greatly improves the thermal conductivity and flame retardant properties of the rubber composite material. Through vinyl trimethoxysilane modification and plasma modification, the compatibility and dispersibility of the granular thermal conductive flame retardant filler with components such as natural rubber and styrene-butadiene rubber are improved.

[0019] Preferably, the plasticizer is one or more of paraffin oil, vaseline and petroleum asphalt.

[0020] Preferably, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 3-5:6:1.

[0021] By adopting the above technical scheme, the role and synergistic effect of the coupling agent are as follows: Promote the interaction between rubber and filler: The coupling agent can react chemically with the rubber matrix resin and the surface of fillers such as two-dimensional sheet-shaped thermal conductive fillers and granular thermal conductive flame retardant fillers to form chemical bonds, enhance the interaction between rubber and fillers, and improve the dispersion of fillers and the reinforcing effect of reinforcing agents. Through the cross-linking reaction between the rubber matrix and the filler, the coupling agent can improve the thermal stability and aging resistance of the composite material and slow down the aging rate of the material. Optimize the thermal conductivity and flame retardant properties of the composite material: The presence of the coupling agent can improve the interface contact between the filler and the rubber matrix, enhance the heat conduction path, and improve the thermal conductivity. At the same time, the coupling agent can also improve the dispersibility of the granular thermal conductive flame retardant filler and its compatibility with the rubber matrix, further improving the flame retardant properties of the composite material. In summary, the coupling agent plays a role in promoting the interaction between rubber and filler, improving the strength and hardness of the rubber, improving the heat resistance and aging resistance, and optimizing the thermal conductivity and flame retardant properties in the high thermal conductivity rubber composite material.

[0022] Preferably, the active agent is composed of zinc oxide and polyacrylamide in a mass ratio of 6:1.

[0023] By adopting the above technical solution, the active agent polyacrylamide can form a high molecular weight network structure during the rubber processing, increase the viscosity of the rubber, and improve the fluidity and processing performance of the rubber. The presence of the active agent can enhance the strength, hardness and wear resistance of the vulcanized rubber, and improve the mechanical properties of the composite material such as tensile strength and elongation at break. Optimize the thermal conductivity and flame retardant properties of the composite material: The active agent can promote the interaction between the two-dimensional flaky thermal conductive filler and the granular thermal conductive flame retardant filler and the rubber matrix resin, enhance the dispersion of the filler and the reinforcing effect of the reinforcing agent, thereby improving the thermal conductivity and flame retardant properties of the composite material.

[0024] Preferably, the antioxidant is at least one of N-phenyl-2-naphthalimide and N-octyl-2-naphthalimide; and the vulcanizing agent is sulfur.

[0025] Preferably, the accelerator is composed of 2-thiol benzothiazole, dibenzothiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0026] By adopting the above technical scheme, the accelerators 2-thiol benzothiazole and dibenzothiazole disulfide are commonly used vulcanizing agent accelerators, which can synergize with the vulcanizing agent to increase the vulcanization reaction rate, promote the vulcanization reaction of the composite material, and accelerate the crosslinking rate of the rubber. Accelerator TMTM is a vulcanizing agent activity enhancer that can increase the activity of the vulcanizing agent and antioxidant in the vulcanization system, enhance the vulcanization crosslinking effect of the rubber, and improve the mechanical properties and heat resistance of the composite material. The presence of the accelerator can improve the aging resistance of the rubber, inhibit the occurrence of aging phenomena such as oxidation, vulcanization fracture and thermal fission, and extend the service life of the composite material. The combination of the three accelerators can play a synergistic role, increase the vulcanization reaction rate and crosslinking effect, and promote the rubber molecules in the composite material to better interact with other components, thereby enhancing the performance of the composite material.

[0027] In a second aspect, the present application provides a method for preparing a high thermal conductivity rubber composite material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned high thermal conductivity rubber composite material, comprising the following steps:

[0028] S101, according to the mass fraction, the natural rubber, styrene-butadiene rubber and plasticizer are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between the two rollers for plastication for 20-25min, and then the coupling agent, the activating agent, the stearic acid, the antioxidant and the accelerator are added step by step in sequence for mixing for 5-8min, after being evenly dispersed, the two-dimensional sheet-like thermal conductive filler and the granular thermal conductive flame retardant filler are added, and after the addition is completed, the mixture is cut and turned over for 5 times, and finally the vulcanizing agent is added, and after mixing is evenly, the mixture is thinned for 6-8 times, the rubber is pounded and the rubber is sliced ​​to obtain a mixed rubber, which is aged for standby use;

[0029] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 155-165° C., pre-compression pressure 8-10 MPa, vulcanization pressure 15-17 MPa, vulcanization time 8-12 min, to obtain a high thermal conductivity rubber composite material.

[0030] In summary, the beneficial technical effects of this application are:

[0031] 1. Excellent thermal conductivity: By adding two-dimensional flake thermal conductive fillers and granular thermal conductive flame retardant fillers, the thermal conductivity of rubber composite materials has been successfully improved. The two-dimensional flake thermal conductive fillers form a continuous three-dimensional thermal conductive filler network in the rubber matrix resin, and the granular thermal conductive flame retardant fillers are evenly dispersed in the silicone rubber matrix resin, so that heat can be conducted and dissipated more effectively, enhancing the thermal conductivity of the material.

[0032] 2. Good flame retardant performance: The introduction of granular thermally conductive flame retardant fillers improves the flame retardant performance of the composite material. The combination of aluminum nitride and magnesium hydroxide can effectively retard flames, and through vinyl trimethoxysilane modification and plasma modification, the compatibility and dispersibility of the filler and the rubber matrix resin are improved, further improving the flame retardant performance.

[0033] 3. Excellent mechanical properties: The reasonable proportion and optimized performance of natural rubber and styrene-butadiene rubber, plasticizers, coupling agents and other components in the composite material make the composite material perform well in mechanical properties. It has good tensile strength, elastic modulus and compressive resistance, and can meet the use requirements in various fields.

[0034] 4. Good insulation performance: The rubber material itself has good insulation performance. In addition, the optimization of the raw material ratio and modification process used in this application makes the insulation performance of the composite material more outstanding, which can well meet the insulation performance requirements of consumer electronics, new energy vehicles, LED lighting and other fields.

[0035] 5. Simple preparation process, fast vulcanization speed, energy saving and environmental protection: The preparation raw materials and process used in this application are relatively simple, and the vulcanization speed is fast, which can greatly improve production efficiency. In addition, the materials and raw materials used in the composite material meet environmental protection requirements and can reduce pollution to the environment. DETAILED DESCRIPTION

[0036] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] Preparation Example 1 Preparation of two-dimensional sheet-like thermal conductive filler

[0038] The preparation method of the two-dimensional sheet-shaped thermal conductive filler comprises the following steps:

[0039] S31, according to the mass parts, 0.15 kg of vinyl trimethoxy silane, 20 kg of isopropanol and 20 kg of water were mixed and stirred to obtain a mixture A;

[0040] S32, adding 8 kg of flake boron nitride, 3 kg of flake graphite and 1 kg of flake aluminum oxide to mixture A according to their mass fractions; then heating to 42° C. and stirring at a speed of 300 r / min for 120 min to obtain a silanized two-dimensional flake thermal conductive filler mixed liquid;

[0041] S33. Filter the silanized two-dimensional flaky thermally conductive filler mixture, wash with ethanol, dry and grind at 75°C, and then perform plasma surface modification for 20 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a two-dimensional flaky thermally conductive filler. The two-dimensional flaky thermally conductive filler has an average radial size of 10 μm and an average thickness of 80 nm.

[0042] Preparation Example 2 Preparation of two-dimensional sheet-like thermal conductive filler

[0043] The preparation method of the two-dimensional sheet-shaped thermal conductive filler comprises the following steps:

[0044] S31, according to the mass parts, 0.15 kg of vinyl trimethoxy silane, 20 kg of isopropanol and 20 kg of water were mixed and stirred to obtain a mixture A;

[0045] S32, adding 8 kg of flake boron nitride, 3 kg of flake graphite and 3 kg of flake aluminum oxide to mixture A according to their mass fractions; then heating to 42° C. and stirring at a speed of 300 r / min for 120 min to obtain a silanized two-dimensional flake thermal conductive filler mixed liquid;

[0046] S33. Filter the silanized two-dimensional flaky thermally conductive filler mixture, wash with ethanol, dry and grind at 75°C, and then perform plasma surface modification for 20 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a two-dimensional flaky thermally conductive filler, wherein the two-dimensional flaky thermally conductive filler has an average radial size of 20 μm and an average thickness of 200 nm.

[0047] Preparation Example 3 Preparation of two-dimensional sheet-like thermal conductive filler

[0048] The preparation method of the two-dimensional sheet-shaped thermal conductive filler comprises the following steps:

[0049] S31, according to the mass parts, 0.15 kg of vinyl trimethoxy silane, 20 kg of isopropanol and 20 kg of water were mixed and stirred to obtain a mixture A;

[0050] S32, adding 8 kg of flake boron nitride, 3 kg of flake graphite and 2 kg of flake aluminum oxide to mixture A according to their mass fractions; then heating to 42° C. and stirring at a speed of 300 r / min for 120 min to obtain a silanized two-dimensional flake thermal conductive filler mixed liquid;

[0051] S33. Filter the silanized two-dimensional flaky thermally conductive filler mixture, wash with ethanol, dry and grind at 75°C, and then perform plasma surface modification for 20 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a two-dimensional flaky thermally conductive filler. The two-dimensional flaky thermally conductive filler has an average radial size of 16 μm and an average thickness of 120 nm.

[0052] Preparation Example 4 Preparation of granular thermally conductive flame retardant filler

[0053] The preparation method of the granular heat-conductive flame-retardant filler comprises the following steps:

[0054] S41, according to the mass parts, 0.2 kg of vinyl trimethoxy silane, 20 kg of isopropanol and 20 kg of water were mixed and stirred to obtain a mixture B;

[0055] S42, adding 10 kg of aluminum nitride and 10 kg of magnesium hydroxide to mixture B according to their mass fractions; then heating to 45° C. and stirring at a speed of 200 r / min for 150 min to obtain a silanized granular thermally conductive flame-retardant filler mixed liquid;

[0056] S43. Filter the silanized granular thermally conductive flame-retardant filler mixture, wash with ethanol, dry at 75°C, grind, and then perform plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a granular thermally conductive flame-retardant filler with an average particle size of 5 μm.

[0057] Preparation Comparative Example 1

[0058] Same as Preparation Example 3, except that the reaction was not modified by plasma.

[0059] Preparation Comparative Example 2

[0060] Same as Preparation Example 4, except that the reaction was not modified by plasma.

[0061] Example 1

[0062] A high thermal conductivity rubber composite material, comprising the following raw materials, by mass: 4.5 kg natural rubber, 4.5 kg styrene-butadiene rubber, 1 kg paraffin oil, 0.2 kg coupling agent, 3 kg two-dimensional flaky thermal conductive filler, 3 kg granular thermal conductive flame retardant filler, 0.5 kg activator, 0.2 kg stearic acid, 0.1 kg N-phenyl-2-naphthalimide, 0.1 kg accelerator, and 0.1 kg sulfur, wherein the two-dimensional flaky thermal conductive filler is the two-dimensional thermal conductive filler prepared in Preparation Example 1. The granular thermally conductive flame-retardant filler is the granular thermally conductive flame-retardant filler prepared in Preparation Example 4, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 3:6:1; the active agent is composed of zinc oxide and polyacrylamide in a mass ratio of 6:1, and the accelerator is composed of 2-thiolbenzothiazole, diphenylthiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0063] The method for preparing the above-mentioned high thermal conductivity rubber composite material comprises the following steps:

[0064] S101, according to the mass fraction, natural rubber, styrene-butadiene rubber and paraffin oil are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plastication for 20 minutes, and then a coupling agent, an activator, stearic acid, N-phenyl-2-naphthalimide and an accelerator are added step by step in sequence for mixing for 5 minutes, after being evenly dispersed, a two-dimensional sheet-like thermal conductive filler and a granular thermal conductive flame-retardant filler are added, and after the addition is completed, the mixture is cut and turned over for 5 times, and finally sulfur is added. After mixing is uniform, the mixture is thinned for 6 times, and the rubber is pounded and sliced ​​to obtain a mixed rubber, which is aged for standby use;

[0065] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 155° C., pre-compression pressure 8 MPa, vulcanization pressure 15 MPa, vulcanization time 8 min, to obtain a high thermal conductivity rubber composite material.

[0066] Example 2

[0067] A high thermal conductivity rubber composite material, comprising the following raw materials by weight: 5 kg natural rubber, 5 kg styrene-butadiene rubber, 1.2 kg vaseline, 0.3 kg coupling agent, 3.5 kg two-dimensional sheet-like thermal conductive filler, 3.5 kg granular thermal conductive flame retardant filler, 0.8 kg activator, 0.4 kg stearic acid, 0.15 kg N-octyl-2-naphthalimide, 0.15 kg accelerator, 0.2 kg sulfur, wherein the two-dimensional sheet-like thermal conductive filler is prepared in Preparation Example 2 The two-dimensional flaky thermally conductive filler is the granular thermally conductive flame-retardant filler prepared in Preparation Example 4, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 5:6:1; the active agent is composed of zinc oxide and polyacrylamide in a mass ratio of 6:1, and the accelerator is composed of 2-thiolbenzothiazole, diphenylthiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0068] The method for preparing the above-mentioned high thermal conductivity rubber composite material comprises the following steps:

[0069] S101, according to the mass fraction, natural rubber, styrene-butadiene rubber and vaseline are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plastication for 25 minutes, and then a coupling agent, an activator, stearic acid, N-octyl-2-naphthalimide and an accelerator are added step by step in sequence for mixing for 8 minutes, after being evenly dispersed, a two-dimensional sheet-like thermal conductive filler and a granular thermal conductive flame-retardant filler are added, and after the addition is completed, the mixture is cut and turned over for 5 times, and finally sulfur is added. After mixing is uniform, the mixture is thinned 8 times, the rubber is pounded and sliced ​​to obtain a mixed rubber, which is aged for standby use;

[0070] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 165° C., pre-compression pressure 10 MPa, vulcanization pressure 17 MPa, vulcanization time 12 min, to obtain a high thermal conductivity rubber composite material.

[0071] Example 3

[0072] A high thermal conductivity rubber composite material, comprising the following raw materials by weight: 4.8 kg natural rubber, 4.8 kg styrene-butadiene rubber, 1.1 kg petroleum asphalt, 0.25 kg coupling agent, 3.3 kg two-dimensional flaky thermal conductive filler, 3.3 kg granular thermal conductive flame retardant filler, 0.7 kg activator, 0.3 kg stearic acid, 0.13 kg N-phenyl-2-naphthalimide, 0.13 kg accelerator, 0.15 kg sulfur, wherein the two-dimensional flaky thermal conductive filler is prepared The two-dimensional flaky thermally conductive filler prepared in Example 3; the granular thermally conductive flame-retardant filler is the granular thermally conductive flame-retardant filler prepared in Preparation Example 4, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 4:6:1; the active agent is composed of zinc oxide and polyacrylamide in a mass ratio of 6:1, and the accelerator is composed of 2-thiolbenzothiazole, diphenylthiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0073] The method for preparing the above-mentioned high thermal conductivity rubber composite material comprises the following steps:

[0074] S101, according to the mass fraction, natural rubber, styrene-butadiene rubber and petroleum asphalt are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plastication for 23 minutes, and then a coupling agent, an activator, stearic acid, N-phenyl-2-naphthalimide and an accelerator are added step by step in sequence for mixing for 7 minutes, and after being evenly dispersed, a two-dimensional sheet-like thermal conductive filler and a granular thermal conductive flame-retardant filler are added, and after the addition is completed, the mixture is cut and turned over for 5 times, and finally sulfur is added, and after mixing is evenly, the mixture is thinned 7 times, and the rubber is pounded and sliced ​​to obtain a mixed rubber, which is aged for standby use;

[0075] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 160° C., pre-compression pressure 9 MPa, vulcanization pressure 16 MPa, vulcanization time 10 min, to obtain a high thermal conductivity rubber composite material.

[0076] Example 4

[0077] The same as Example 3, except that an equal amount of γ-aminopropyltriethoxysilane is used to replace the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 4:6:1.

[0078] Example 5

[0079] The same as Example 3, except that an equal amount of vinyltrimethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 4:6:1.

[0080] Example 6

[0081] The same as Example 3, except that an equal amount of γ-mercaptopropyltriethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 4:6:1.

[0082] Example 7

[0083] The same as Example 3, except that an equal amount of 2-thiol benzothiazole is used to replace the accelerator, and the accelerator is composed of 2-thiol benzothiazole, dibenzothiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0084] Example 8

[0085] The same as Example 3, except that an equal amount of diphenylthiazole disulfide is used to replace the accelerator, and the accelerator is composed of 2-thiol benzothiazole, diphenylthiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0086] Example 9

[0087] The same as Example 3, except that an equal amount of accelerator TMTM is used to replace the accelerator, and the accelerator is composed of 2-thiol benzothiazole, dibenzothiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5.

[0088] Comparative Example 1

[0089] The same as Example 3, except that an equal amount of the two-dimensional sheet-like thermally conductive filler prepared in Preparation Comparative Example 1 is used to replace the two-dimensional sheet-like thermally conductive filler prepared in Preparation Example 3. An equal amount of the granular thermally conductive flame-retardant filler prepared in Preparation Comparative Example 2 is used to replace the granular thermally conductive flame-retardant filler prepared in Preparation Example 4.

[0090] Comparative Example 2

[0091] The same as Example 3, except that an equal amount of flaky boron nitride (the average radial dimension of the flaky boron nitride is 16 μm and the average thickness is 120 nm) is used to replace the two-dimensional flaky thermal conductive filler prepared in Preparation Example 3.

[0092] Comparative Example 3

[0093] The same as Example 3, except that an equal amount of flaky graphite sheets (the average radial dimension of the flaky graphite sheets is 16 μm and the average thickness is 120 nm) is used to replace the two-dimensional flaky thermal conductive filler prepared in Preparation Example 3.

[0094] Comparative Example 4

[0095] The same as Example 3, except that an equal amount of flaky aluminum oxide (the average radial size of the flaky aluminum oxide is 16 μm and the average thickness is 120 nm) is used to replace the two-dimensional flaky thermal conductive filler prepared in Preparation Example 3.

[0096] Performance Testing

[0097] The high thermal conductivity rubber composite materials prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were sampled and tested. The test results are shown in Table 1.

[0098] Thermal resistance: Refer to "ASTM D 5470-06 Standard Test Method for Thermal Transfer Performance of Thermally Conductive Electrical Insulating Materials" and use LW-9389 thermal resistance meter for testing;

[0099] Thermal conductivity: Refer to "GB / T32064-2015 Transient Plane Heat Source Test Method for Thermal Conductivity and Thermal Diffusivity of Building Materials", and use TPS2500S thermal constant analyzer for testing;

[0100] Shore hardness: refer to "GB / T531.1-2008 Test method for indentation hardness of vulcanized rubber or thermoplastic rubber Part 1: Shore hardness tester method (Shore hardness)", and use CLZ-AC Shore hardness tester for testing;

[0101] Volume resistivity: Refer to "GB / T 31838.2-2019 Dielectric and resistance properties of solid insulating materials Part 2: Resistance characteristics (DC method) Volume resistance and volume resistivity", and use PC40B high insulation resistance meter for testing;

[0102] Breakdown voltage strength: refer to "GB / T 1695-2005 Determination of power frequency breakdown voltage strength and withstand voltage of vulcanized rubber", and use 125B withstand voltage tester for testing;

[0103] Flame retardant grade: Refer to "GB / T 10707-2008 Determination of combustion performance of rubber", and use UL94 vertical and horizontal combustion test machine for testing.

[0104] Table 1 Performance test

[0105]

[0106]

[0107] Analyzing the data in Table 1, we can see that:

[0108] 1) The high thermal conductivity rubber composite material prepared in Examples 1 to 3 has good thermal conductivity, good flame retardancy, good insulation, low thermal resistance and breakdown resistance, and its preparation process is simple, the vulcanization speed is fast, and it is energy-saving and environmentally friendly. It can well meet the thermal conductivity and heat dissipation needs of consumer electronics, new energy vehicles, LED lighting and other fields.

[0109] 2) By comparing the performance of the high thermal conductivity rubber composite materials obtained in Example 3 and Example 4-Example 6, a coupling agent consisting of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and γ-mercaptopropyltriethoxysilane in a mass ratio of 4:6:1 is used, and the synergistic effect between them is utilized to improve the comprehensive performance of the high thermal conductivity rubber composite material.

[0110] 3) A comparative analysis of the performance of a high thermal conductivity rubber composite material was obtained by combining Example 3 with Examples 7 to 9. The accelerator is composed of 2-thiolbenzothiazole, dibenzothiazole disulfide and accelerator TMTM in a mass ratio of 2:1:5. The synergistic effect between them is utilized to increase the vulcanization reaction rate and the crosslinking effect, and promote the rubber molecules in the composite material to better interact with other components, thereby enhancing the performance of the composite material.

[0111] 4) Based on the comparative analysis of the performance of the high thermal conductivity rubber composite materials obtained in Example 3 and Comparative Example 1, the two-dimensional flaky thermal conductive filler and the granular thermal conductive flame retardant filler are modified by oxygen plasma to improve the interface compatibility, thereby improving the comprehensive performance of the high thermal conductivity rubber composite material.

[0112] 5) In combination with the performance comparison analysis of the high thermal conductivity rubber composite materials prepared in Example 3 and Comparative Examples 2-4, the two-dimensional flaky thermal conductive filler prepared in Preparation Example 3 is used, and the synergistic effect between flaky boron nitride, flaky graphite sheets and flaky aluminum oxide and vinyl trimethoxysilane modification are utilized, and then plasma modification treatment is performed to form a continuous three-dimensional thermal conductive filler network in the rubber matrix resin, which significantly improves the thermal conductivity of the high thermal conductivity rubber composite material. Through vinyl trimethoxysilane modification and plasma modification, its compatibility and dispersibility with the rubber matrix are improved, and the comprehensive performance of the high thermal conductivity rubber composite material is further improved.

[0113] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A high thermal conductivity rubber composite material, characterized in that: The preparation material comprises the following raw materials by weight: 45-50 parts of natural rubber, 45-50 parts of styrene-butadiene rubber, 10-12 parts of plasticizer, 2-3 parts of coupling agent, 30-35 parts of two-dimensional flaky thermal conductive filler, 30-35 parts of granular thermal conductive flame retardant filler, 5-8 parts of active agent, 2-4 parts of stearic acid, 1-1.5 parts of antioxidant, 1-1.5 parts of accelerator and 1-2 parts of vulcanizer, wherein the two-dimensional flaky thermal conductive filler is composed of flaky boron nitride, flaky graphite and flaky aluminum oxide in a weight ratio of 8:3:1-3, and is modified by vinyltrimethoxysilane and then plasma modified; the granular thermal conductive flame retardant filler is composed of aluminum nitride and magnesium hydroxide in a weight ratio of 1:1, and is modified by vinyltrimethoxysilane and then plasma modified; the mass fraction ratio of the two-dimensional flaky thermal conductive filler to the granular thermal conductive flame retardant filler is 1:

1.

2. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The average radial dimension of the two-dimensional flaky thermally conductive filler is 10-20 μm, and the average thickness is 80-200 nm; the average particle size of the granular thermally conductive flame-retardant filler is 1-10 μm.

3. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The method for preparing the two-dimensional sheet-shaped thermal conductive filler comprises the following steps: S31, according to the weight ratio, 1.5 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed and stirred to obtain a mixture A; S32, adding 80 parts of flaky boron nitride, 30 parts of flaky graphite sheets and 10-30 parts of flaky aluminum oxide to mixture A according to their weight percentages; then heating to 42° C. and stirring at a speed of 300 r / min for 120 min to obtain a silanized two-dimensional flaky thermal conductive filler mixed liquid; S33. Filter the silanized two-dimensional flaky thermally conductive filler mixture, wash with ethanol, dry and grind at 75°C, and then perform plasma surface modification for 20 seconds at a power of 2KW and an oxygen volume concentration of 10% to obtain a two-dimensional flaky thermally conductive filler, wherein the two-dimensional flaky thermally conductive filler has an average radial size of 10-20μm and an average thickness of 80-200nm.

4. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The method for preparing the granular thermally conductive flame-retardant filler comprises the following steps: S41, according to the mass parts, 2 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed, and stirred to obtain a mixture B; S42, adding 100 parts of aluminum nitride and 100 parts of magnesium hydroxide to mixture B according to their mass fractions; then raising the temperature to 45° C. and stirring at a speed of 200 r / min for 150 min to obtain a silanized granular thermally conductive flame-retardant filler mixed liquid; S43. Filter the silanized granular thermally conductive flame-retardant filler mixture, wash with ethanol, dry at 75°C, grind, and then perform plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a granular thermally conductive flame-retardant filler with an average particle size of 1-10 μm.

5. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The plasticizer is one or more of paraffin oil, vaseline and petroleum asphalt.

6. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The coupling agent is composed of gamma-aminopropyltriethoxysilane, vinyltrimethoxysilane and gamma-mercaptopropyltriethoxysilane in a mass ratio of 3-5:6:

1.

7. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The active agent is composed of zinc oxide and polyacrylamide in a mass ratio of 6:

1.

8. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The antioxidant is at least one of N-phenyl-2-naphthalene imide and N-octyl-2-naphthalene imide; and the vulcanizing agent is sulfur.

9. The high thermal conductivity rubber composite material according to claim 1, characterized in that: The accelerator is composed of 2-thiol benzothiazole, dibenzothiazole disulfide and accelerator TMTM in a mass ratio of 2:1:

5.

10. A method for preparing a high thermal conductivity rubber composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, according to the mass fraction, the natural rubber, styrene-butadiene rubber and plasticizer are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between the two rollers for plastication for 20-25min, and then the coupling agent, the activating agent, the stearic acid, the antioxidant and the accelerator are added step by step in sequence for mixing for 5-8min, after being evenly dispersed, the two-dimensional sheet-like thermal conductive filler and the granular thermal conductive flame retardant filler are added, and after the addition is completed, the mixture is cut and turned over for 5 times, and finally the vulcanizing agent is added, and after mixing is evenly, the mixture is thinned for 6-8 times, the rubber is pounded and the rubber is sliced ​​to obtain a mixed rubber, which is aged for standby use; S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 155-165° C., pre-compression pressure 8-10 MPa, vulcanization pressure 15-17 MPa, vulcanization time 8-12 min, to obtain a high thermal conductivity rubber composite material.

Citation Information

Patent Citations

  • Heat-conducting silicone rubber composite material as well as preparation method and application thereof

    CN116285354A

  • High-performance rubber composite material and preparation method thereof

    CN116589764A

Cited By

  • Preparation method of core-shell type heat-conducting particle composite ethylene propylene diene monomer thermal interface material

    CN120157963A