A method for preparing thickening powder for powder coating
By combining the concave and convex rod soil with aniline and modified carboxymethyl cellulose, a powder coating thickening powder with thickening and antibacterial properties was prepared, which solved the problem of the lack of antibacterial properties of the existing powder coating thickening powder, and achieved more Long service life and environmentally friendly low-energy consumption process.
Patent Information
- Application Number
- CN202410589798.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-13
AI Technical Summary
The existing powder coating thickening powder lacks antibacterial properties, which leads to the coating being prone to mildew, has a short service life, and is complex in traditional preparation processes, high cost, and has a large pollution, making it difficult to meet the needs of environmental protection and low energy consumption.
Polyaniline composite polyaniline soil is used to synthesize polyaniline composite polyaniline soil, and carboxymethyl cellulose is modified through chitosan and berberine to form antibacterial modified powder components, combined with silane coupling agent and sodium hydroxide to neutralize Acrylic acid, powder coating thickening powder with thickening and antibacterial properties is prepared through dry mixing, grinding and ultrasonic dispersion.
The prepared powder coating thickening powder not only has good thickening properties, but also has stable antibacterial properties, which can effectively prevent mold and extend the service life of the coating, while simplifying the process flow and reducing energy consumption and pollution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thickening powder preparation methods, and in particular to a method for preparing thickening powder for powder coatings. Background Art
[0002] As a new type of environmentally friendly coating, powder coating has occupied an increasingly important position in the coating market due to its advantages such as solvent-free, low pollution, easy recycling and convenient construction. However, with the continuous expansion of the application field of powder coating, the performance requirements are also increasing. Among them, the viscosity control of the coating is one of the key factors to ensure the quality of coating construction. Thickening powder is a key auxiliary agent for adjusting the viscosity of the coating, and its preparation method has an important influence on the performance of powder coating.
[0003] At present, the powder coating thickeners on the market are mainly prepared by two methods: physical mixing and chemical synthesis. Although the physical mixing method is simple to operate, it has problems such as uneven mixing and unstable thickening effect; the chemical synthesis method can obtain thickeners with more stable performance, but the preparation process is complicated, the cost is high, and it may involve the use of toxic and hazardous substances. In addition, with the increasing awareness of environmental protection, the coating industry has an increasingly urgent demand for low-pollution, low-energy consumption, and high-efficiency preparation processes. Most of the existing powder coating thickeners only focus on their thickening properties, and other properties such as antibacterial properties need to be improved. If the powder coating thickener is improved to have better antibacterial properties, the probability of mildew of the coating can be greatly reduced, thereby extending the service life of the coating. Therefore, those skilled in the art are in urgent need of designing a new powder coating thickener so that it can have stable antibacterial properties on the basis of having a good thickening effect. Summary of the invention
[0004] Technical issues solved
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing a thickening powder for powder coatings, which can effectively solve the problem that the thickening powder for powder coatings in the prior art does not have antibacterial properties.
[0006] Technical Solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for preparing a thickening powder for a powder coating, the method comprising the following steps:
[0009] S1. preparing polyaniline composite attapulgite using attapulgite and aniline as raw materials;
[0010] S2, modifying carboxymethyl cellulose with chitosan to prepare antibacterial modified carboxymethyl cellulose, and then modifying carboxymethyl cellulose with berberine to prepare berberine-modified carboxymethyl cellulose;
[0011] S3, weighing polyaniline composite attapulgite, antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose in a weight ratio of 5:1:1, dry-mixing, grinding and passing through a 200-mesh sieve to record as a powder component;
[0012] S4, mixing the powder component and the silane coupling agent solution in a weight ratio of 1:5, and concentrating to 1 / 3 of the original volume after ultrasonic dispersion, and the obtained powder component is recorded as a modified powder component;
[0013] S5, weighing 2-3 g of the modified powder component and mixing it with 50-60 mL of acrylic acid neutralized with sodium hydroxide, stirring at a stirring speed of 1000 r / min for 10 min, adding 2 g of ammonium persulfate, and stirring the mixture at a temperature of 70° C. for 4-5 h to obtain a colloidal composite;
[0014] S6. Place the colloidal compound in an oven at 65°C and dry for 12 hours. Grind the compound through a 100-mesh sieve to obtain a powder coating thickening powder.
[0015] Furthermore, in S1, the preparation method of polyaniline composite attapulgite is:
[0016] 1) Grind the attapulgite through a 200-mesh sieve and soak it in deionized water. Centrifuge it at 5000 r / min for 5 min, remove the supernatant, and dry the precipitate in a vacuum drying oven at 65°C for 12 h. Then disperse it in deionized water again, and ultrasonically disperse it at a frequency of 28-29 kHz for 5 min to prepare a attapulgite slurry with a mass concentration of 20%.
[0017] 2) Weigh 0.01 mol of calculated amount of ammonium persulfate and 18-20 mL of attapulgite slurry and pour them into a reactor. Add 2 mL of aniline and stir at 200 r / min for 4 h at room temperature. Filter and remove the filtrate, wash with deionized water for 3 times, and dry in a vacuum drying oven at 80°C for 12 h to obtain polyaniline composite attapulgite.
[0018] Furthermore, in S2, the preparation method of the antibacterial modified carboxymethyl cellulose is as follows: 5g of carboxymethyl cellulose is weighed and dispersed in 100mL of deionized water, and the dispersion is evenly allowed to stand for 12 hours, and the result is recorded as the carboxymethyl cellulose component; 3g of chitosan and 5g of anhydrous calcium chloride are weighed and dissolved in 100mL of glacial acetic acid aqueous solution, and the dispersion is evenly allowed to stand for 12 hours, and then the carboxymethyl cellulose component is added dropwise, stirred at a stirring speed of 100r / min for 30 minutes, and then freeze-dried, and the result is the antibacterial modified carboxymethyl cellulose.
[0019] Furthermore, in the preparation method of antibacterial modified carboxymethyl cellulose, the stirring speed for uniform dispersion is 500 r / min, the stirring time for uniform dispersion is 5 min, the volume concentration of the glacial acetic acid aqueous solution is 2%, and the dripping rate is 2 drops / s.
[0020] Furthermore, in S2, the preparation steps of the berberine-treated carboxymethyl cellulose are:
[0021] Step 1, weigh 1g of carboxymethyl cellulose and disperse it in 20mL of deionized water, stir at a stirring speed of 1500r / min for 12h, then add 10mL of sodium metaperiodate aqueous solution, stir evenly and adjust the pH value to 3, stir at the original stirring speed for 4h under light-proof conditions, then add 50mL of anhydrous ethanol for precipitation, wash the obtained precipitate with anhydrous ethanol 3 times and then freeze-dry, and the obtained product is dialdehyde carboxymethyl cellulose;
[0022] Step 2, weigh 8g of berberine and 16mL of 2,4-dimethoxybenzylamine, pour them into a flask, stir them at a temperature of 120°C and a stirring speed of 1500r / min for 8h, wash them with acetone after cooling and freeze-dry them to obtain the product, weigh 3g of the product, dissolve it in 30mL of methanol and add 3mL of concentrated hydrochloric acid, stir it at a stirring speed of 500r / min for 6h, filter it, and finally wash the precipitate with an ethanol aqueous solution and freeze-dry it. The obtained product is recorded as modified berberine;
[0023] Step 3, weigh 1.5 g of dialdehyde carboxymethyl cellulose and 3 g of modified berberine, pour them into 200 mL of deionized water, adjust the pH value to 5, stir at 40° C., and stir at a speed of 1500 r / min for 12 h. The resultant product after freeze-drying is berberine carboxymethyl cellulose.
[0024] Furthermore, in step 1, the concentration of the sodium metaperiodate aqueous solution is 0.11 g / mL, the stirring speed for uniform stirring is 300 r / min, the stirring time for uniform stirring is 10 min, and the pH value is adjusted using a 1 mol / L sulfuric acid aqueous solution. In step 2, the mass fraction of concentrated hydrochloric acid is 35%, the volume concentration of the ethanol aqueous solution is 80%, and in step 3, the pH value is adjusted using a 1 mol / L sulfuric acid aqueous solution.
[0025] Furthermore, in S3, the stirring speed of the dry mixing is 300 r / min, and the stirring time of the dry mixing is 10 min.
[0026] Furthermore, in S4, the preparation method of the silane coupling agent solution is: 5-8 parts by weight of silane coupling agent KH-560 is added to 50 parts by weight of deionized water, and stirred at a stirring speed of 500 r / min for 5 minutes.
[0027] Furthermore, in S4, the frequency of ultrasonic dispersion is 26-28 kHz, and the time of ultrasonic dispersion is 5 min.
[0028] Furthermore, in S5, the preparation method of acrylic acid neutralized with sodium hydroxide is: weigh 7g of acrylic acid and 7g of acrylamide, pour them into a flask, add 20mL of 6mol / L sodium hydroxide aqueous solution under ice water bath conditions, and mix them. In S5, the stirring speed of the stirring reaction is 300r / min.
[0029] Beneficial Effects
[0030] The present invention provides a method for preparing a thickening powder for powder coatings. Compared with the prior art, the present invention has the following beneficial effects:
[0031] In the present invention, attapulgite is modified by polyaniline having good thermal stability, so that its stability can be improved and the prepared polyaniline composite attapulgite has better dispersibility. After modification with acrylic acid and acrylamide, the thickening effect of the prepared powder coating thickening powder can be improved. Combined with the thickening performance and antibacterial performance of antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose, the powder coating thickening powder prepared by the present invention can have excellent mildew resistance on the basis of having good thickening performance.
[0032] The present invention modifies carboxymethyl cellulose with chitosan having antibacterial properties, so that a polyelectrolyte complex is formed between chitosan and carboxymethyl cellulose through ionic bonds, and the prepared antibacterial modified carboxymethyl cellulose has good stability and antibacterial properties; secondly, the carboxymethyl cellulose is modified with berberine, and during the modification process, the lone pair of electrons on the amino group of the modified berberine attacks the carbon group on the dialdehyde carboxymethyl cellulose, so that a stable chemical bond is formed between berberine and carboxymethyl cellulose, and the prepared berberine carboxymethyl cellulose has stable antibacterial properties; finally, the antibacterial properties of the antibacterial modified carboxymethyl cellulose and the berberine carboxymethyl cellulose cooperate with each other, and the prepared thickening powder has stable antibacterial properties. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention will be further described below in conjunction with the embodiments.
[0035] Example 1
[0036] A method for preparing a thickening powder for a powder coating according to the present embodiment comprises the following steps:
[0037] S1. Polyaniline composite attapulgite is prepared using attapulgite and aniline as raw materials.
[0038] S2. Carboxymethyl cellulose is modified with chitosan to prepare antibacterial modified carboxymethyl cellulose, and then carboxymethyl cellulose is modified with berberine to prepare berberine-modified carboxymethyl cellulose.
[0039] S3. Weigh polyaniline composite attapulgite, antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose in a weight ratio of 5:1:1, dry-mix them, grind them and pass through a 200-mesh sieve to record them as powder components; the stirring speed of the dry mixing is 300 r / min, and the stirring time of the dry mixing is 10 min.
[0040] S4. Mix the powder component and the silane coupling agent solution in a weight ratio of 1:5, concentrate to 1 / 3 of the original volume after ultrasonic dispersion, and record the result as modified powder component; wherein, the preparation method of the silane coupling agent solution is: add 5 parts by weight of silane coupling agent KH-560 to 50 parts by weight of deionized water, and stir at a stirring speed of 500 r / min for 5 minutes; the frequency of ultrasonic dispersion is 26 kHz, and the time of ultrasonic dispersion is 5 minutes.
[0041] S5. Weigh 2 g of the modified powder component and mix it with 50 mL of acrylic acid neutralized with sodium hydroxide, stir it at a stirring speed of 1000 r / min for 10 min, then add 2 g of ammonium persulfate, and stir it at a stirring speed of 300 r / min at a temperature of 70°C for 4 h to obtain a colloidal complex; the preparation method of acrylic acid neutralized with sodium hydroxide is as follows: weigh 7 g of acrylic acid and 7 g of acrylamide, pour them into a flask, add 20 mL of a 6 mol / L sodium hydroxide aqueous solution in an ice water bath, and mix them.
[0042] S6. Place the colloidal compound in an oven at 65°C and dry for 12 hours. Grind the compound through a 100-mesh sieve to obtain a powder coating thickening powder.
[0043] In S1, the preparation method of polyaniline composite attapulgite is:
[0044] 1) Grind the attapulgite through a 200-mesh sieve and soak it in deionized water. Centrifuge it at 5000 r / min for 5 min, remove the supernatant, and dry the precipitate in a vacuum drying oven at 65°C for 12 h. Then disperse it in deionized water again, and ultrasonically disperse it at a frequency of 28 kHz for 5 min to prepare a attapulgite slurry with a mass concentration of 20%.
[0045] 2) Weigh 0.01 mol of calculated amount of ammonium persulfate and 18 mL of attapulgite slurry and pour them into a reactor. Add 2 mL of aniline and stir at 200 r / min for 4 h at room temperature. Filter and remove the filtrate, wash with deionized water for 3 times, and dry in a vacuum drying oven at 80°C for 12 h to obtain polyaniline composite attapulgite.
[0046] In S2, the preparation method of antibacterial modified carboxymethyl cellulose is as follows: weigh 5g of carboxymethyl cellulose and disperse it in 100mL of deionized water, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h. The result is recorded as the carboxymethyl cellulose component; weigh 3g of chitosan and 5g of anhydrous calcium chloride and dissolve them in 100mL of 2% volume concentration of glacial acetic acid aqueous solution, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h, then add the carboxymethyl cellulose component at a dripping rate of 2 drops / s, stir it at a stirring speed of 100r / min for 30min, and then freeze-dry it. The result is the antibacterial modified carboxymethyl cellulose.
[0047] In S2, the preparation steps of berberine carboxymethyl cellulose are:
[0048] Step 1, weigh 1g of carboxymethyl cellulose and disperse it in 20mL of deionized water, stir at a stirring speed of 1500r / min for 12h, then add 10mL of 0.11g / mL sodium metaperiodate aqueous solution, stir at a stirring speed of 300r / min for 10min, adjust the pH value to 3 with a 1mol / L sulfuric acid aqueous solution, stir at the original stirring speed for 4h under light-proof conditions, then add 50mL of anhydrous ethanol for precipitation, wash the obtained precipitate 3 times with anhydrous ethanol and then freeze-dry, and the obtained product is dialdehyde carboxymethyl cellulose;
[0049] Step 2, weigh 8g of berberine and 16mL of 2,4-dimethoxybenzylamine, pour them into a flask, stir them at a temperature of 120°C and a stirring speed of 1500r / min for 8h, wash them with acetone after cooling and freeze-dry them to obtain a product, weigh 3g of the product, dissolve it in 30mL of methanol and add 3mL of 35% concentrated hydrochloric acid by mass, stir it at a stirring speed of 500r / min for 6h, filter it, and finally wash the precipitate with an ethanol aqueous solution with a volume concentration of 80% and freeze-dry it. The obtained product is recorded as modified berberine;
[0050] Step 3, weigh 1.5 g of dialdehyde carboxymethyl cellulose and 3 g of modified berberine, pour them into 200 mL of deionized water, adjust the pH value to 5 with a 1 mol / L sulfuric acid aqueous solution, stir at 40 ° C at a stirring speed of 1500 r / min for 12 h, and freeze-dry to obtain berberine carboxymethyl cellulose.
[0051] Example 2
[0052] A method for preparing a thickening powder for a powder coating according to the present embodiment comprises the following steps:
[0053] S1. Polyaniline composite attapulgite is prepared using attapulgite and aniline as raw materials.
[0054] S2. Carboxymethyl cellulose is modified with chitosan to prepare antibacterial modified carboxymethyl cellulose, and then carboxymethyl cellulose is modified with berberine to prepare berberine-modified carboxymethyl cellulose.
[0055] S3. Weigh polyaniline composite attapulgite, antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose in a weight ratio of 5:1:1, dry-mix them, grind them and pass through a 200-mesh sieve to record them as powder components; the stirring speed of the dry mixing is 300 r / min, and the stirring time of the dry mixing is 10 min.
[0056] S4. Mix the powder component and the silane coupling agent solution in a weight ratio of 1:5, concentrate to 1 / 3 of the original volume after ultrasonic dispersion, and record the result as modified powder component; wherein, the preparation method of the silane coupling agent solution is: add 8 parts by weight of silane coupling agent KH-560 to 50 parts by weight of deionized water, and stir at a stirring speed of 500 r / min for 5 minutes; the frequency of ultrasonic dispersion is 28 kHz, and the time of ultrasonic dispersion is 5 minutes.
[0057] S5. Weigh 3 g of the modified powder component and mix it with 60 mL of acrylic acid neutralized with sodium hydroxide, stir it at a stirring speed of 1000 r / min for 10 min, then add 2 g of ammonium persulfate, and stir it at a stirring speed of 300 r / min at a temperature of 70°C for 5 h to obtain a colloidal complex; the preparation method of acrylic acid neutralized with sodium hydroxide is as follows: weigh 7 g of acrylic acid and 7 g of acrylamide, pour them into a flask, add 20 mL of a 6 mol / L sodium hydroxide aqueous solution in an ice water bath, and mix them.
[0058] S6. Place the colloidal compound in an oven at 65°C and dry for 12 hours. Grind the compound through a 100-mesh sieve to obtain a powder coating thickening powder.
[0059] In S1, the preparation method of polyaniline composite attapulgite is:
[0060] 1) Grind the attapulgite through a 200-mesh sieve and soak it in deionized water. Centrifuge it at 5000 r / min for 5 min, remove the supernatant, and dry the precipitate in a vacuum drying oven at 65°C for 12 h. Then disperse it in deionized water again, and ultrasonically disperse it at a frequency of 29 kHz for 5 min to prepare a attapulgite slurry with a mass concentration of 20%.
[0061] 2) Weigh 0.01 mol of calculated amount of ammonium persulfate and 20 mL of attapulgite slurry and pour them into a reactor. Add 2 mL of aniline and stir at 200 r / min for 4 h at room temperature. Filter and remove the filtrate, wash with deionized water for 3 times, and dry in a vacuum drying oven at 80 °C for 12 h to obtain polyaniline composite attapulgite.
[0062] In S2, the preparation method of antibacterial modified carboxymethyl cellulose is as follows: weigh 5g of carboxymethyl cellulose and disperse it in 100mL of deionized water, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h. The result is recorded as the carboxymethyl cellulose component; weigh 3g of chitosan and 5g of anhydrous calcium chloride and dissolve them in 100mL of 2% volume concentration of glacial acetic acid aqueous solution, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h, then add the carboxymethyl cellulose component at a dripping rate of 2 drops / s, stir it at a stirring speed of 100r / min for 30min, and then freeze-dry it. The result is the antibacterial modified carboxymethyl cellulose.
[0063] In S2, the preparation steps of berberine carboxymethyl cellulose are:
[0064] Step 1, weigh 1g of carboxymethyl cellulose and disperse it in 20mL of deionized water, stir at a stirring speed of 1500r / min for 12h, then add 10mL of 0.11g / mL sodium metaperiodate aqueous solution, stir at a stirring speed of 300r / min for 10min, adjust the pH value to 3 with a 1mol / L sulfuric acid aqueous solution, stir at the original stirring speed for 4h under light-proof conditions, then add 50mL of anhydrous ethanol for precipitation, wash the obtained precipitate 3 times with anhydrous ethanol and then freeze-dry, and the obtained product is dialdehyde carboxymethyl cellulose;
[0065] Step 2, weigh 8g of berberine and 16mL of 2,4-dimethoxybenzylamine, pour them into a flask, stir them at a temperature of 120°C and a stirring speed of 1500r / min for 8h, wash them with acetone after cooling and freeze-dry them to obtain a product, weigh 3g of the product, dissolve it in 30mL of methanol and add 3mL of 35% concentrated hydrochloric acid by mass, stir it at a stirring speed of 500r / min for 6h, filter it, and finally wash the precipitate with an ethanol aqueous solution with a volume concentration of 80% and freeze-dry it. The obtained product is recorded as modified berberine;
[0066] Step 3, weigh 1.5 g of dialdehyde carboxymethyl cellulose and 3 g of modified berberine, pour them into 200 mL of deionized water, adjust the pH value to 5 with a 1 mol / L sulfuric acid aqueous solution, stir at 40 ° C at a stirring speed of 1500 r / min for 12 h, and freeze-dry to obtain berberine carboxymethyl cellulose.
[0067] Example 3
[0068] A method for preparing a thickening powder for a powder coating according to the present embodiment comprises the following steps:
[0069] S1. Polyaniline composite attapulgite is prepared using attapulgite and aniline as raw materials.
[0070] S2. Carboxymethyl cellulose is modified with chitosan to prepare antibacterial modified carboxymethyl cellulose, and then carboxymethyl cellulose is modified with berberine to prepare berberine-modified carboxymethyl cellulose.
[0071] S3. Weigh polyaniline composite attapulgite, antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose in a weight ratio of 5:1:1, dry-mix them, grind them and pass through a 200-mesh sieve to record them as powder components; the stirring speed of the dry mixing is 300 r / min, and the stirring time of the dry mixing is 10 min.
[0072] S4. Mix the powder component and the silane coupling agent solution in a weight ratio of 1:5, concentrate to 1 / 3 of the original volume after ultrasonic dispersion, and record the result as modified powder component; wherein, the preparation method of the silane coupling agent solution is: add 7 parts by weight of silane coupling agent KH-560 to 50 parts by weight of deionized water, and stir at a stirring speed of 500 r / min for 5 minutes; the frequency of ultrasonic dispersion is 27 kHz, and the time of ultrasonic dispersion is 5 minutes.
[0073] S5. Weigh 3 g of the modified powder component and mix it with 55 mL of acrylic acid neutralized with sodium hydroxide, stir it at a stirring speed of 1000 r / min for 10 min, then add 2 g of ammonium persulfate, and stir it at a stirring speed of 300 r / min at a temperature of 70°C for 5 h to obtain a colloidal complex; the preparation method of acrylic acid neutralized with sodium hydroxide is as follows: weigh 7 g of acrylic acid and 7 g of acrylamide, pour them into a flask, add 20 mL of a 6 mol / L sodium hydroxide aqueous solution in an ice water bath, and mix them.
[0074] S6. Place the colloidal compound in an oven at 65°C and dry for 12 hours. Grind the compound through a 100-mesh sieve to obtain a powder coating thickening powder.
[0075] In S1, the preparation method of polyaniline composite attapulgite is:
[0076] 1) Grind the attapulgite through a 200-mesh sieve and soak it in deionized water. Centrifuge it at 5000 r / min for 5 min, remove the supernatant, and dry the precipitate in a vacuum drying oven at 65°C for 12 h. Then disperse it in deionized water again, and ultrasonically disperse it at a frequency of 29 kHz for 5 min to prepare a attapulgite slurry with a mass concentration of 20%.
[0077] 2) Weigh 0.01 mol of calculated amount of ammonium persulfate and 19 mL of attapulgite slurry and pour them into a reactor. Add 2 mL of aniline and stir at 200 r / min for 4 h at room temperature. Filter and remove the filtrate, wash with deionized water for 3 times, and dry in a vacuum drying oven at 80 °C for 12 h to obtain polyaniline composite attapulgite.
[0078] In S2, the preparation method of antibacterial modified carboxymethyl cellulose is as follows: weigh 5g of carboxymethyl cellulose and disperse it in 100mL of deionized water, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h. The result is recorded as the carboxymethyl cellulose component; weigh 3g of chitosan and 5g of anhydrous calcium chloride and dissolve them in 100mL of 2% volume concentration of glacial acetic acid aqueous solution, stir it at a stirring speed of 500r / min for 5min, and then let it stand for 12h, then add the carboxymethyl cellulose component at a dripping rate of 2 drops / s, stir it at a stirring speed of 100r / min for 30min, and then freeze-dry it. The result is the antibacterial modified carboxymethyl cellulose.
[0079] In S2, the preparation steps of berberine carboxymethyl cellulose are:
[0080] Step 1, weigh 1g of carboxymethyl cellulose and disperse it in 20mL of deionized water, stir at a stirring speed of 1500r / min for 12h, then add 10mL of 0.11g / mL sodium metaperiodate aqueous solution, stir at a stirring speed of 300r / min for 10min, adjust the pH value to 3 with a 1mol / L sulfuric acid aqueous solution, stir at the original stirring speed for 4h under light-proof conditions, then add 50mL of anhydrous ethanol for precipitation, wash the obtained precipitate 3 times with anhydrous ethanol and then freeze-dry, and the obtained product is dialdehyde carboxymethyl cellulose;
[0081] Step 2, weigh 8g of berberine and 16mL of 2,4-dimethoxybenzylamine, pour them into a flask, stir them at a temperature of 120°C and a stirring speed of 1500r / min for 8h, wash them with acetone after cooling and freeze-dry them to obtain a product, weigh 3g of the product, dissolve it in 30mL of methanol and add 3mL of 35% concentrated hydrochloric acid by mass, stir it at a stirring speed of 500r / min for 6h, filter it, and finally wash the precipitate with an ethanol aqueous solution with a volume concentration of 80% and freeze-dry it. The obtained product is recorded as modified berberine;
[0082] Step 3, weigh 1.5 g of dialdehyde carboxymethyl cellulose and 3 g of modified berberine, pour them into 200 mL of deionized water, adjust the pH value to 5 with a 1 mol / L sulfuric acid aqueous solution, stir at 40 ° C at a stirring speed of 1500 r / min for 12 h, and freeze-dry to obtain berberine carboxymethyl cellulose.
[0083] Comparative Example 1
[0084] The preparation method of a powder coating thickener provided in this comparative example is substantially the same as that in Example 1, the main difference being that in this comparative example 1, the polyaniline composite attapulgite in Example 1 is replaced with unmodified attapulgite.
[0085] Comparative Example 2
[0086] The preparation method of a powder coating thickener provided in this comparative example is substantially the same as that in Example 1, the main difference being that in this comparative example 1, the antibacterial modified carboxymethyl cellulose in Example 1 is replaced with unmodified carboxymethyl cellulose.
[0087] Comparative Example 3
[0088] The preparation method of a powder coating thickener provided in this comparative example is substantially the same as that in Example 1, the main difference being that in this comparative example 1, the berberine-modified carboxymethyl cellulose in Example 1 is replaced with unmodified carboxymethyl cellulose.
[0089] Performance Testing
[0090] The powder coating thickening powders prepared in Examples 1-3 and Comparative Examples 1-3 are marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-3 is tested. The specific testing methods and test items are as follows:
[0091] 1. The powder coating thickening powder prepared in Example 1-3 and Comparative Example 1-3 was mixed with n-butanol at a material-liquid ratio of 1:12, and the viscosity was tested after stirring at a speed of 60 r / min for 5 minutes. The obtained data were recorded in the following table;
[0092] 2. Add the powder coating thickener prepared in Examples 1-3 and Comparative Examples 1-3 to the sterilized culture medium at an addition amount of 50 mg / mL, disperse by ultrasonication for 15 minutes, and then use a pipette to transfer the diluted bacterial suspension (Escherichia coli) to the test solution. A group without the powder coating thickener is used as a positive control and placed in a 37°C constant temperature incubator for shaking culture for 20 hours. After culturing for 20 hours, use a pipette to take out 200 µL of the culture solution to an ELISA plate (take two copies of each sample in parallel), measure its absorbance (OD630 value) on an ELISA reader with a wavelength of 630 nm, and calculate its antibacterial rate according to the following formula.
[0093] Antibacterial rate (%) = (positive control OD value - sample OD value) / positive control OD value × 100%
[0094]
[0095] The data in the above table show that the viscosity of the powder coating thickening powder in Examples 1-3 is significantly higher than that in Comparative Example 1, indicating that the addition of polyaniline composite attapulgite in the preparation raw material has a better viscosity than the unmodified attapulgite, thereby being able to better increase the viscosity of the coating; secondly, the antibacterial rate of the powder coating thickening powder in Examples 1-3 is significantly higher than that in Comparative Examples 2-3, indicating that the antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose cooperate with each other to achieve better antibacterial performance. Therefore, the powder coating thickening powder prepared in the present invention has better market promotion value.
[0096] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a thickening powder for powder coatings, It is characterized in that The preparation method comprises the following steps: S1. preparing polyaniline composite attapulgite using attapulgite and aniline as raw materials; S2, modifying carboxymethyl cellulose with chitosan to prepare antibacterial modified carboxymethyl cellulose, and then modifying carboxymethyl cellulose with berberine to prepare berberine-modified carboxymethyl cellulose; S3, weighing polyaniline composite attapulgite, antibacterial modified carboxymethyl cellulose and berberine carboxymethyl cellulose in a weight ratio of 5:1:1, dry-mixing, grinding and passing through a 200-mesh sieve to record as a powder component; S4, mixing the powder component and the silane coupling agent solution in a weight ratio of 1:5, and concentrating to 1 / 3 of the original volume after ultrasonic dispersion, and the obtained powder component is recorded as a modified powder component; S5, weighing 2-3 g of the modified powder component and mixing it with 50-60 mL of acrylic acid neutralized with sodium hydroxide, stirring at a stirring speed of 1000 r / min for 10 min, adding 2 g of ammonium persulfate, and stirring the mixture at a temperature of 70° C. for 4-5 h to obtain a colloidal composite; S6, drying the colloidal compound in an oven at 65°C for 12 hours, and grinding the compound through a 100-mesh sieve to obtain a powder coating thickening powder; In S1, the preparation method of polyaniline composite attapulgite is: 1) Grind the attapulgite through a 200-mesh sieve and soak it in deionized water. Centrifuge it at 5000 r / min for 5 min, remove the supernatant, and dry the precipitate in a vacuum drying oven at 65°C for 12 h. Then disperse it in deionized water again, and ultrasonically disperse it at a frequency of 28-29 kHz for 5 min to prepare a attapulgite slurry with a mass concentration of 20%. 2) Weigh 0.01 mol of calculated amount of ammonium persulfate and 18-20 mL of attapulgite slurry into a reactor, add 2 mL of aniline and stir at 200 r / min for 4 h at room temperature, filter to remove the filtrate and wash with deionized water for 3 times, place in a vacuum drying oven at 80 ° C and dry for 12 h, and the obtained product is polyaniline composite attapulgite; In S2, the preparation method of the antibacterial modified carboxymethyl cellulose is as follows: 5g of carboxymethyl cellulose is weighed and dispersed in 100mL of deionized water, and the dispersion is uniform and then allowed to stand for 12 hours, and the obtained product is recorded as the carboxymethyl cellulose component; 3g of chitosan and 5g of anhydrous calcium chloride are weighed and dissolved in 100mL of glacial acetic acid aqueous solution, and the dispersion is uniform and then allowed to stand for 12 hours, and then the carboxymethyl cellulose component is added dropwise, and the mixture is stirred at a stirring speed of 100r / min for 30min and then freeze-dried, and the obtained product is the antibacterial modified carboxymethyl cellulose; In S2, the preparation steps of the berberine carboxymethyl cellulose are: Step 1, weigh 1g of carboxymethyl cellulose and disperse it in 20mL of deionized water, stir at a stirring speed of 1500r / min for 12h, then add 10mL of sodium metaperiodate aqueous solution, stir evenly and adjust the pH value to 3, stir at the original stirring speed for 4h under light-proof conditions, then add 50mL of anhydrous ethanol for precipitation, wash the obtained precipitate with anhydrous ethanol 3 times and then freeze-dry, and the obtained product is dialdehyde carboxymethyl cellulose; Step 2, weigh 8g of berberine and 16mL of 2,4-dimethoxybenzylamine, pour them into a flask, stir them at a temperature of 120°C and a stirring speed of 1500r / min for 8h, wash them with acetone after cooling and freeze-dry them to obtain the product, weigh 3g of the product, dissolve it in 30mL of methanol and add 3mL of concentrated hydrochloric acid, stir it at a stirring speed of 500r / min for 6h, filter it, and finally wash the precipitate with an ethanol aqueous solution and freeze-dry it. The obtained product is recorded as modified berberine; Step 3, weighing 1.5 g of dialdehyde carboxymethyl cellulose and 3 g of modified berberine, pouring into 200 mL of deionized water, adjusting the pH value to 5, stirring at 40° C. and 1500 r / min for 12 h, and freeze-drying to obtain berberine carboxymethyl cellulose; In S5, the preparation method of acrylic acid neutralized with sodium hydroxide is: weigh 7g of acrylic acid and 7g of acrylamide, pour them into a flask, add 20mL of 6mol / L sodium hydroxide aqueous solution under ice water bath condition, and mix them. In S5, the stirring speed of the stirring reaction is 300r / min.
2. A method for preparing a thickening powder for powder coatings according to claim 1, It is characterized in that In the preparation method of antibacterial modified carboxymethyl cellulose, the stirring speed for uniform dispersion is 500 r / min, the stirring time for uniform dispersion is 5 min, the volume concentration of the glacial acetic acid aqueous solution is 2%, and the dripping rate is 2 drops / s.
3. The method for preparing a thickening powder for powder coating according to claim 1, It is characterized in that In step 1, the concentration of the sodium metaperiodate aqueous solution is 0.11 g / mL, the stirring speed for uniform stirring is 300 r / min, the stirring time for uniform stirring is 10 min, and the pH value is adjusted using a 1 mol / L sulfuric acid aqueous solution. In step 2, the mass fraction of concentrated hydrochloric acid is 35%, and the volume concentration of the ethanol aqueous solution is 80%. In step 3, the pH value is adjusted using a 1 mol / L sulfuric acid aqueous solution.
4. The method for preparing a thickening powder for powder coating according to claim 1, It is characterized in that In S3, the stirring speed of dry mixing is 300 r / min, and the stirring time of dry mixing is 10 min.
5. The method for preparing a thickening powder for powder coating according to claim 1, It is characterized in that In S4, the silane coupling agent solution is prepared by adding 5-8 parts by weight of silane coupling agent KH-560 to 50 parts by weight of deionized water, and stirring at a speed of 500 r / min for 5 minutes.
6. The method for preparing a thickening powder for powder coating according to claim 1, It is characterized in that In S4, the frequency of ultrasonic dispersion is 26-28 kHz, and the time of ultrasonic dispersion is 5 min.