A glue-filled power supply shell

By applying a thermal coating on the power supply shell, using modified thermal filler I and modified thermal filler II, the problem of delamination of the potting glue from the power supply shell is solved, the adhesion and thermal conductivity are improved, and the service life of the power supply is extended .

CN118222172BActive Publication Date: 2024-11-15CHANGZHOU CHUANGLIAN POWER SUPPLY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410314371.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-15
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

The existing potting glue is delaminated from the power shell under high and low temperature hot and cold cycles, resulting in insufficient heat dissipation, affecting the service life of the power supply, and lacks methods to effectively improve the adhesion of silicone potting glue to substrates.

Method used

Using a thermally conductive coating, the modified thermally conductive filler I and modified thermally conductive filler II are formulated to form an elastic thermally conductive coating, which enhances adhesion to the shell and sealant, and compensates for the expansion of the sealant during the hot and cold cycle. improve thermal conductivity.

Benefits of technology

It realizes excellent adhesion and elasticity of the thermal coating on the power supply case, improves thermal conductivity and mechanical properties, and extends the service life of the power supply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004748501690000291
    Figure BDA0004748501690000291
  • Figure BDA0004748501690000301
    Figure BDA0004748501690000301
Patent Text Reader

Abstract

The present invention belongs to the field of functional coatings, and specifically relates to a glue-filled power supply shell, including a power supply shell, wherein the inner surface of the power supply shell is coated with a thermal conductive coating, and the thermal conductive coating comprises the following raw materials in parts by weight: 40.0-60.0 parts of polyurethane acrylate prepolymer, 5.0-10.0 parts of modified thermal conductive filler I, 1.5-3.0 parts of modified thermal conductive filler II, 8.0-15.0 parts of UV monomer diluent, 2.0-5.0 parts of photoinitiator, 0.1-0.4 parts of leveling agent, and organic solvent remainder, and the total amount of each component is 100 parts. The thermal conductive coating is obtained through a paint making process, a coating process, and curing. The thermal conductive coating of the present invention is designed by formula, and is matched with homemade modified thermal conductive filler I and modified thermal conductive filler II, which can effectively improve the problem of insufficient heat dissipation effect caused by delamination of sealant and power supply shell in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional coatings, and in particular relates to a glue-filled power supply shell. Background Art

[0002] Electronic component potting glue has many functions such as heat dissipation, moisture resistance, and insect resistance. It is a conventional means of protecting electronic components. Commonly used potting glues include epoxy potting glue, polyurethane potting glue, and silicone potting glue. Epoxy potting glue has high viscosity, poor permeability, and is easy to crack; while polyurethane potting glue has poor high temperature resistance, many bubbles, and poor construction performance. Silicone potting glue, especially addition-type silicone potting glue, has its unique advantages in electronic module potting. It is safe and environmentally friendly, does not release heat during curing, does not release small molecules, has good deep curing, low curing shrinkage, small internal stress, and little damage to precision electronic components. At the same time, the cross-linking density and curing speed are easy to control, and the application process performance is excellent. In particular, its cured product has excellent high and low temperature resistance and can be used for a long time at -60-250℃. It is widely used in communication electronics, solar energy, LED, automobiles, aerospace and other fields.

[0003] Of course, silicone potting glue also has some shortcomings compared to epoxy potting glue and polyurethane potting glue. For example, the adhesion of silicone potting glue to the substrate is relatively weak. During long-term use, due to the high and low temperature hot and cold cycles, the potting glue will delaminate from the power supply shell, resulting in the heat dissipation of electronic components being blocked, thus affecting the service life of the power supply.

[0004] In recent years, the research focus of scientific researchers has been on how to improve the adhesion of silicone potting glue to the substrate and further improve the thermal conductivity of the potting glue. This has great practical significance. However, there is little research on pre-treatment of the power shell to improve the adhesion between the silicone potting glue and the substrate. Summary of the invention

[0005] The purpose of the present invention is to provide a thermally conductive coating and a preparation method thereof in view of the fact that a glue-filled power supply shell and sealant in the prior art have debonding phenomenon after high and low temperature cold and hot cycles, resulting in insufficient heat dissipation. Through formula design, as well as homemade modified thermally conductive filler I and modified thermally conductive filler II, an elastic thermally conductive coating is formed after a painting process and UV curing. On the one hand, it has excellent adhesion to the shell material and sealant, and on the other hand, it also has excellent elasticity to compensate for the expansion rate of the sealant in the cold and hot cycles. In order to achieve the above purpose, the technical solution adopted by the present invention to solve its technical problems is as follows:

[0006] A glue-filled power supply shell comprises a power supply shell, wherein the inner surface of the power supply shell is coated with a thermal conductive coating.

[0007] Specifically, the thermal conductive coating comprises the following raw materials in parts by weight:

[0008] 40.0-60.0 parts of polyurethane acrylate prepolymer;

[0009] Modified thermally conductive filler I 5.0-10.0 parts;

[0010] Modified thermal conductive filler II 1.5-3.0 parts;

[0011] UV monomer diluent 8.0-15.0 parts;

[0012] Photoinitiator 2.0-5.0 parts;

[0013] Leveling agent 0.1-0.4 parts;

[0014] Residue of organic solvent;

[0015] The total amount of the above components is 100 parts.

[0016] Specifically, the modified thermally conductive filler I and the modified thermally conductive filler II are mixed at a mass ratio of 3.0-4.0:1.

[0017] Specifically, the preparation method of the modified thermally conductive filler I comprises the following steps:

[0018] (1) placing metal oxide A and aminosilane coupling agent in an alcohol solvent to carry out silylation coupling reaction to prepare intermediate product I;

[0019] (2) intermediate product I is subjected to a condensation reaction with asymmetric diisocyanate A to prepare intermediate product II;

[0020] (3) the intermediate product II is subjected to a condensation reaction with a diol in the presence of a catalyst, dibutyltin dilaurate A, to prepare an intermediate product III;

[0021] (4) the intermediate product III is subjected to a condensation reaction with an asymmetric diisocyanate B in the presence of a catalyst, dibutyltin dilaurate B, to prepare an intermediate product IV;

[0022] (5) The intermediate product IV undergoes a condensation reaction with graphene oxide in the presence of a catalyst, dibutyltin dilaurate C, to obtain the target product, i.e., the modified thermal conductive filler I.

[0023] Specifically,

[0024] The metal oxide A is a spherical structure;

[0025] The amount of the metal oxide A, aminosilane coupling agent, and alcohol solvent is 1g: 3.3-5.5g: 80mL;

[0026] The usage ratio of the intermediate product I and the asymmetric diisocyanate A is 4.3-6.5 g: 0.015-0.025 mol;

[0027] The diol is a polyether diol or a polyester diol;

[0028] The intermediate product II and diol are added in a molar ratio of isocyanate to hydroxyl of 1:2;

[0029] The amount of dibutyltin dilaurate A is 1.0-1.5wt% of the total mass of the reactants;

[0030] The intermediate product III and the asymmetric diisocyanate B are added at a molar ratio of hydroxyl to isocyanate of 1:2;

[0031] The amount of dibutyltin dilaurate B is 1.0-1.5wt% of the total mass of the reactants;

[0032] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0033] The graphene oxide is graphene oxide prepared by improving Hummer's method; and

[0034] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0035] Specifically, the preparation method of the modified thermally conductive filler II comprises the following steps:

[0036] (1) placing metal oxide B and mercaptosilane coupling agent in an alcohol solvent to carry out silylation coupling reaction to prepare intermediate product 1;

[0037] (2) intermediate product 1 undergoes a "thiol-ene" click reaction with vinyl silicone oil to prepare intermediate product 2;

[0038] (3) The intermediate product 2 is reacted with hydrogen-containing silicone oil in the presence of a catalyst, chloroplatinic acid, to undergo a hydrosilylation reaction to obtain the target product, i.e., the modified thermal conductive filler II.

[0039] Specifically, the metal oxide B is a needle-shaped or whisker structure;

[0040] The amount of the metal oxide B, mercaptosilane coupling agent, and alcohol solvent is 1g: 3.3-5.5g: 80mL;

[0041] The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group; and

[0042] The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of 1:2 between vinyl and silicon hydrogen.

[0043] Specifically, the preparation method of the thermal conductive coating is:

[0044] Protect from light, keep humidity ≤60%, mix the leveling agent and organic solvent evenly, then add polyurethane acrylate prepolymer, UV monomer diluent, modified thermal conductive filler I and modified thermal conductive filler II to the mixed solvent in sequence, continue to stir evenly, add photoinitiator, stir evenly, filter with filter cloth with a pore size of 1 μm to obtain the thermal conductive coating.

[0045] A method for preparing a glue-filled power supply housing comprises the following steps:

[0046] The thermal conductive coating according to any one of claims 1 to 8 is uniformly coated on the inner surface of the power supply housing, the solvent is removed by heating, and the coating layer is subjected to UV irradiation to obtain a glue-filled power supply housing.

[0047] Specifically, the power supply casing is a metal power supply casing.

[0048] The present invention has the following beneficial effects:

[0049] (1) The present invention provides a thermally conductive coating, the main resin of which is a polyurethane acrylate prepolymer. On the one hand, the polyurethane acrylate prepolymer has relatively high flexibility; on the other hand, the polyurethane structure also has high adhesion to various substrates.

[0050] (2) The present invention provides a thermally conductive coating, wherein one of its components is a modified thermally conductive filler I, which contains metal oxide, silane, polyurethane structure, and graphene structure in its molecular structure; and the metal oxide and graphene are connected by a flexible organic chain to form a "hyperbranched beaded" structure. First, the metal oxide and graphene have high thermal conductivity, which is conducive to the heat dissipation of the glue-filled power supply; second, the contact surface between the spherical metal oxide and the flaky graphene structure is maximized, which is conducive to the propagation of phonons and further improves the thermal conductivity; third, the polyurethane structure between the metal oxide microspheres and the graphene is composed of soft and hard segments and has excellent flexibility; fourth, the core-shell structure formed by the spherical metal oxide wrapped by the organic chain and the flaky graphene layers can slide relative to each other, further improving the flexibility of the coating; fifth, the polyurethane wrapped structure is conducive to the dispersibility and compatibility in the polyurethane acrylate system; sixth, the silane structure has a certain high temperature resistance on the one hand; on the other hand, it can improve the compatibility with the modified thermally conductive filler II and improve the mechanical and thermal properties.

[0051] (3) The present invention provides a thermally conductive coating, one of the components of which is a modified thermally conductive filler II, which contains metal oxides, long-chain siloxane structures and silicon hydrogen structures in its molecular structure. First, the long-chain siloxane structure has good compatibility with the silane of the modified thermally conductive filler I, thereby improving the thermal conductivity; second, the needle-shaped or whisker-shaped metal oxide has anisotropy and can be dispersed between the layers and rings of epoxy graphene, as well as between the spherical metal oxides to act as a "bridge", making the entire thermal surface larger and more three-dimensional, and having a higher thermal conductivity; third, the long-chain siloxane structure has excellent high and low temperature resistance and flexibility; fourth, the residual silicon hydrogen structure in the structure can react with the sealant (silicon-based addition type AB glue) when the power supply is glued, thereby improving the adhesion between the sealant and the coating, and avoiding debonding in high and low temperature environments, which is of great significance to improving the heat dissipation of the power supply.

[0052] Thus, the thermally conductive coating of the present invention, which is a compound of modified thermally conductive filler I and modified thermally conductive filler II, has excellent thermal conductivity, and also has excellent elasticity and adhesion, and can meet the normal use of the current glue-filled power supply shell. DETAILED DESCRIPTION

[0053] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0054] The purpose of the present invention is to develop a coating with excellent adhesion and bonding to the power shell and good flexibility to meet its use on the glue-filled power shell. The idea of ​​realization is: to make one or more additives with excellent thermal conductivity, and at the same time, they have high flexibility, or have excellent flexibility together with the main resin. The theoretical basis of realization is: first, prepare a modified thermal conductive filler I, through metal oxides and graphene with high thermal conductivity, wrap it through a flexible polyurethane structure, and at the same time meet the requirements of its dispersibility in the subject resin; wherein the metal oxide is a spherical structure, ensuring that it has more contact surface with the layered graphene. Second, prepare a modified thermal conductive filler II, through needle-shaped or whisker-shaped metal oxides as a "bridge", the spherical metal oxides and graphene are more likely to be linked, and a more three-dimensional spatial thermal conductive network is obtained; in addition, the modified thermal conductive filler II contains an organic silicon chain structure and residual silicon-hydrogen bonds, so that the modified thermal conductive filler II has excellent compatibility and reactivity with the organic silicon glue, improves the adhesion of the organic silicon glue on the coating, and has the flexibility of the organic silicon chain. At the same time, the modified thermally conductive filler I and the modified thermally conductive filler II are compatible due to the entanglement of macromolecule chains, and the modified thermally conductive filler I is compatible with the polyurethane acrylate system, and the overall compatibility is excellent. The modified thermally conductive filler I and the modified thermally conductive filler II in the present invention complement each other, synergistically enhance the effect, and have excellent thermal conductivity and flexibility. The embodiments of the present invention are as follows:

[0055] The embodiment of the present invention provides a method for preparing a modified thermally conductive filler I, comprising the following steps:

[0056] (1) adding metal oxide A and aminosilane coupling agent to an alcohol solvent, subjecting to ultrasonic oscillation for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 2-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product I;

[0057] The usage ratio of the metal oxide A, aminosilane coupling agent and alcohol solvent is 1g:3.5-5.5g:80mL;

[0058] The metal oxide A described in the present invention has a spherical structure, is spherical aluminum oxide, has an average particle size of 30 nm, and is purchased from Beasley New Materials (Suzhou) Co., Ltd.

[0059] The silane coupling agent in the present invention is an aminosilane coupling agent, which can be KH901, KH902, KH540, KH550, KH602, KH792; and KH550 is preferred;

[0060] The alcohol solvent in the present invention can be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.

[0061] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring to disperse, and then adding the mixture dropwise to N,N-dimethylformamide B containing asymmetric diisocyanate A through a peristaltic pump, stirring at room temperature for 2-4 hours, and after the reaction is completed, distilling under reduced pressure, and drying under vacuum at 60° C. for 8 hours to obtain the intermediate product II;

[0062] The usage ratio of the intermediate product I, N,N-dimethylformamide A, asymmetric diisocyanate A, and N,N-dimethylformamide B is: 4.3-6.5 g: 100 mL: 0.015-0.025 mol: 200 mL;

[0063] The asymmetric diisocyanate A in the present invention can be isophorone diisocyanate A, toluene diisocyanate A, or L-lysine diisocyanate A.

[0064] The toluene diisocyanate A may be toluene-2,3-diisocyanate, toluene-2,4-diisocyanate, toluene-2,5-diisocyanate or toluene-3,4-diisocyanate; and preferably toluene-2,4-diisocyanate.

[0065] (3) N2 protection, adding the intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing diol by a peristaltic pump, reacting at 60-120° C., and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and dried in vacuum at 80° C. for 4 h to obtain the intermediate product III;

[0066] The intermediate product II and diol are added in a molar ratio of isocyanate to hydroxyl of 1:2;

[0067] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0068] The diol and N,N-dimethylformamide D are used in a ratio of 10 g to 150 mL;

[0069] The amount of dibutyltin dilaurate A used is 1.0-1.5wt% of the total mass of the reactants.

[0070] The diol described in the present invention is a polyether diol or a polyester diol.

[0071] The polyether glycol can be PEG or PPG.

[0072] The PEG is PEG400, PEG600, PEG800, PEG1000, etc.; and preferably, PEG600.

[0073] The PPG is PPG400, PPG600, PPG800, PPG1000, etc.; and preferably, PPG800.

[0074] The polyester diol may be polycaprolactone diol, and its molecular weight may be 400, 530, 830, 1000, 2000, etc., and preferably has a molecular weight of 530.

[0075] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing asymmetric diisocyanate B and dibutyltin dilaurate B by a peristaltic pump, stirring at 40-100° C. for 8-12 h. After the reaction is completed, distillation under reduced pressure is performed, and vacuum drying is performed at 60° C. for 8 h to obtain the intermediate product IV;

[0076] The intermediate product III and the asymmetric diisocyanate B are added at a molar ratio of hydroxyl to isocyanate of 1:2;

[0077] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0078] The usage ratio of the asymmetric diisocyanate B to N,N-dimethylformamide F is 5g:200mL;

[0079] The amount of dibutyltin dilaurate B used is 1.0-1.5wt% of the total mass of the reactants.

[0080] The asymmetric diisocyanate B in the present invention can be isophorone diisocyanate B, toluene diisocyanate B, or L-lysine diisocyanate B.

[0081] The toluene diisocyanate B may be toluene-2,3-diisocyanate, toluene-2,4-diisocyanate, toluene-2,5-diisocyanate or toluene-3,4-diisocyanate; and preferably toluene-2,4-diisocyanate.

[0082] (5) adding graphene oxide to N,N-dimethylformamide G, ultrasonicating for 2 h at 200 W ultrasonic power, adding intermediate product IV and dibutyltin dilaurate C, heating to 60-120 ° C, and determining the reaction end point by infrared detection of isocyanate; after the reaction, filtering and rinsing with dichloromethane, and drying the filter cake in vacuum at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0083] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0084] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0085] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0086] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0087] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0088] The embodiment of the present invention provides a method for preparing a modified thermally conductive filler II, comprising the following steps:

[0089] (1) adding metal oxide B and mercaptosilane coupling agent to an alcohol solvent, subjecting to ultrasonic oscillation for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 4-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain an intermediate product 1;

[0090] The usage ratio of the metal oxide B, mercaptosilane coupling agent and alcohol solvent is 1g:3.5-5.5g:80mL;

[0091] The metal oxide B in the present invention is a needle-shaped or whisker structure, and is a needle-shaped aluminum oxide or magnesium oxide whisker.

[0092] The needle-shaped alumina used in the following examples of the present invention has a particle size of 20-40 nm and is purchased from Shanghai Huijing Sub-Nano New Materials Co., Ltd.

[0093] The magnesium oxide whiskers used in the following embodiments of the present invention have a diameter of 0.1-1 μm and a length of 5-100 μm, and are purchased from Wuhan Kemik Biomedical Technology Co., Ltd.

[0094] The thiol coupling agent in the present invention may be KH580 or KH590; and preferably KH580;

[0095] The alcohol solvent in the present invention can be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.

[0096] (2) N2 protection, the intermediate product 1 is dispersed in N,N-dimethylformamide H, and added dropwise to toluene containing vinyl silicone oil via a peristaltic pump, and the temperature is raised to 30-50°C and stirred for 2-4 hours; vacuum distillation is performed, and vacuum drying is performed at 40°C for 24 hours to obtain the intermediate product 2;

[0097] The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group.

[0098] The usage ratio of the intermediate product 1 to N,N-dimethylformamide H is 10 g:200 mL;

[0099] The usage ratio of the vinyl silicone oil to toluene is 10 g:150 mL;

[0100] The vinyl silicone oil described in the following examples of the present invention is a side chain vinyl silicone oil with a vinyl content of 0.2 wt % and a viscosity of 300 cp, which is purchased from Zhonglan Chenguang Chemical Research Institute.

[0101] (3) The intermediate product 2 is added to tetrahydrofuran, and then added dropwise to toluene containing hydrogenated silicone oil and catalyst chloroplatinic acid via a peristaltic pump, and stirred. After reacting at 70-120° C. for 4-5 hours, the solvent is removed by vacuum distillation, and the mixture is dried at 80° C. in vacuo for 4 hours to obtain the target product, i.e., the modified thermal conductive filler II;

[0102] The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of vinyl to silicon hydrogen of 1:2.

[0103] The usage ratio of the intermediate product 2 to tetrahydrofuran is 10 g:200 mL;

[0104] The usage ratio of the hydrogen-containing silicone oil to toluene is 10 g:300 mL;

[0105] The amount of chloroplatinic acid used is 0.05wt% of the total mass of the reactants.

[0106] The hydrogen-containing silicone oil described in the following examples of the present invention has a hydrogen content of 0.6 wt % and a viscosity of 100 cp, and is purchased from Shandong Dayi Chemical Co., Ltd.

[0107] An embodiment of the present invention provides a thermal conductive coating, comprising the following raw materials in parts by weight:

[0108] 40.0-60.0 parts of polyurethane acrylate prepolymer;

[0109] Modified thermally conductive filler I 5.0-10.0 parts;

[0110] Modified thermal conductive filler II 1.5-3.0 parts;

[0111] UV monomer diluent 8.0-15.0 parts;

[0112] Photoinitiator 2.0-5.0 parts;

[0113] Leveling agent 0.1-0.4 parts;

[0114] Residue of organic solvent;

[0115] The total amount of the above components is 100 parts.

[0116] The polyurethane acrylate prepolymer in the present invention may be one or more of difunctional, trifunctional, and hexafunctional.

[0117] The difunctional polyurethane acrylate prepolymer may be Sartomer CN965, Sartomer CN980, Sartomer CN981, Sartomer CN996, Sartomer CN9001, Sartomer CN9782, Cytec EB270, Corning Photomer 6217, Corning Photomer 6572, Shimei M1800, and the like.

[0118] The trifunctional polyurethane acrylate prepolymer may be Sartomer CN989, Cytec EB205H, Corning Photomer 6892, Zhongshan Qianye Synthetic UV2300, or the like.

[0119] The modified thermally conductive filler I and the modified thermally conductive filler II in the present invention are mixed at a mass ratio of 3.0-4.0:1.

[0120] The UV monomer diluent described in the present invention is any combination of monofunctional, difunctional, trifunctional, tetrafunctional or hexafunctional.

[0121] The monofunctional UV monomer diluent in the present invention may be HEA, IBOMA, EOEOEA, and the like.

[0122] The difunctional UV monomer diluent in the present invention may be PDDA, NPGDA, DPGDA, HDDA, TPGDA, and the like.

[0123] The trifunctional UV monomer diluent in the present invention may be EO-TMPTA, PO-TMPTA, PETA, and the like.

[0124] The tetrafunctional UV monomer diluent in the present invention may be PETTA or the like.

[0125] The hexafunctional UV monomer diluent in the present invention may be dipentaerythritol hexaacrylate or the like.

[0126] The photoinitiator described in the present invention is BP, 184, 1173 or TPO, etc. The photoinitiator described in the following embodiments of the present invention is a mixture of BP and 184 in a mass ratio of 1:2.

[0127] The leveling agent in the present invention is 401LS or Tego 2100, preferably 401LS.

[0128] The organic solvent described in the present invention is one or more of MIBK, EAc, BAc, PM, and PMA. The organic solvent described in the following embodiments of the present invention is a mixture of EAc and PMA in a mass ratio of 2:1.

[0129] A method for preparing a thermally conductive coating in the following embodiment of the present invention comprises the following steps:

[0130] Protect from light, keep humidity ≤60%, mix the leveling agent and organic solvent evenly, then add polyurethane acrylate prepolymer, UV monomer diluent, modified thermal conductive filler I and modified thermal conductive filler II to the mixed solvent in sequence, continue to stir evenly, add photoinitiator, stir evenly, filter with filter cloth with a pore size of 1 μm to obtain the thermal conductive coating.

[0131] The embodiment of the present invention provides a method for preparing a thermal conductive coating for a glue-filled power supply shell, comprising the following steps:

[0132] Under N2 protection, the thermal conductive coating is evenly coated on the substrate, heated at 80°C for 180s, and the coating layer is irradiated with UV light with an irradiation energy of 400-600mJ / cm 2 , the irradiation time is 30-60s, and the glue-filled power supply shell with a dry film thickness of 30-40μm is obtained.

[0133] The substrate described in the present invention is a plastic substrate or a metal substrate. The metal substrate is an iron-based material or an aluminum-based material; and the substrate described in the following embodiments of the present invention is an aluminum-based material that has been sandblasted.

[0134] In order to further understand the present invention, a glue-filled power supply shell provided by the present invention is described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0135] Example 1

[0136] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0137] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0138] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0139] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0140] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0141] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0142] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1:-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0143] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 60°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and vacuum dried at 80°C for 4 hours to obtain intermediate product III;

[0144] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0145] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0146] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0147] The amount of dibutyltin dilaurate A used is 1.0wt% of the total mass of the reactants.

[0148] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0149] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing toluene-2,4-diisocyanate and dibutyltin dilaurate B through a peristaltic pump, stirring at 40°C for 10 hours. After the reaction is completed, vacuum distillation is performed, and vacuum drying is performed at 60°C for 8 hours to obtain the intermediate product IV;

[0150] The intermediate product III and toluene-2,4-diisocyanate are added at a molar ratio of hydroxyl group to isocyanate group of 1:2;

[0151] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0152] The usage ratio of toluene-2,4-diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0153] The amount of dibutyltin dilaurate B used is 1.0 wt% of the total mass of the reactants.

[0154] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0155] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 60 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0156] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0157] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0158] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0159] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0160] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0161] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1:-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0162] A method for preparing a modified thermally conductive filler II comprises the following steps:

[0163] (1) Add magnesium oxide whiskers and mercaptosilane coupling agent KH580 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 70° C. for 6 h, filter, take the insoluble matter, and dry at 60° C. for 12 h to obtain intermediate product 1;

[0164] The dosage ratio of the magnesium oxide whisker, the mercaptosilane coupling agent KH580, and the anhydrous ethanol is 1 g:4.6 g:80 mL.

[0165] Its infrared data is as follows: 3438cm -1 :-OH weakened; 2550cm -1 :-SH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0166] (2) Under N2 protection, the intermediate product 1 was dispersed in N,N-dimethylformamide H, and added dropwise to toluene containing vinyl silicone oil via a peristaltic pump, and the temperature was raised to 40°C and stirred for 3 hours; the intermediate product 2 was obtained by vacuum distillation and vacuum drying at 40°C for 24 hours;

[0167] The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group.

[0168] The usage ratio of the intermediate product 1 to N,N-dimethylformamide H is 10 g:200 mL;

[0169] The usage ratio of the vinyl silicone oil to toluene is 10g:150mL.

[0170] Its infrared data is as follows: 3438cm -1 :-OH exists; 2550cm -1:-SH does not exist; 1625cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0171] (3) The intermediate product 2 was added to tetrahydrofuran, and then added dropwise to toluene containing hydrogenated silicone oil and catalyst chloroplatinic acid via a peristaltic pump, and stirred. After reacting at 100° C. for 4.5 h, the solvent was removed by vacuum distillation, and the mixture was dried at 80° C. for 4 h to obtain the target product, i.e., the modified thermal conductive filler II.

[0172] The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of vinyl to silicon hydrogen of 1:2.

[0173] The usage ratio of the intermediate product 2 to tetrahydrofuran is 10 g:200 mL;

[0174] The usage ratio of the hydrogen-containing silicone oil to toluene is 10 g:300 mL;

[0175] The amount of chloroplatinic acid used is 0.05wt% of the total mass of the reactants.

[0176] Its infrared data is as follows: 3438cm -1 :-OH exists; 2150cm -1 :-Si-H exists; 1625cm -1 :-C=C- does not exist; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0177] A thermal conductive coating comprises the following raw materials in parts by weight:

[0178] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0179] 8.0 parts of modified thermally conductive filler I;

[0180] Modified thermal conductive filler II 2.2 parts;

[0181] TPGDA 4.0 copies;

[0182] PO-TMPTA 4.0 parts;

[0183] PETTA 2.0 parts;

[0184] 3.0 parts of photoinitiator;

[0185] Leveling agent 401LS 0.3 parts;

[0186] Residue of organic solvent;

[0187] The total amount of the above components is 100 parts.

[0188] A method for preparing a glue-filled power supply housing comprises the following steps:

[0189] The thermal conductive coating was evenly coated on the substrate under N2 protection, heated at 80°C for 180s, and the coating layer was irradiated with UV light at an irradiation energy of 500mJ / cm 2 , the irradiation time is 50s, and the glue-filled power supply shell with a dry film thickness of 35μm is obtained.

[0190] Example 2

[0191] The rest is the same as in Example 1, except that:

[0192] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0193] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 80° C. for 2 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain an intermediate product I;

[0194] The dosage ratio of the spherical alumina, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:3.5g:80mL.

[0195] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0196] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0197] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 4.3 g: 100 mL: 0.015 mol: 200 mL.

[0198] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0199] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 60°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and vacuum dried at 80°C for 4 hours to obtain intermediate product III;

[0200] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0201] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0202] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0203] The amount of dibutyltin dilaurate A used is 1.0wt% of the total mass of the reactants.

[0204] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0205] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing toluene-2,4-diisocyanate and dibutyltin dilaurate B through a peristaltic pump, stirring at 40°C for 10 hours. After the reaction is completed, vacuum distillation is performed, and vacuum drying is performed at 60°C for 8 hours to obtain the intermediate product IV;

[0206] The intermediate product III and toluene-2,4-diisocyanate are added at a molar ratio of hydroxyl group to isocyanate group of 1:2;

[0207] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0208] The usage ratio of toluene-2,4-diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0209] The amount of dibutyltin dilaurate B used is 1.0 wt% of the total mass of the reactants.

[0210] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0211] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 60 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0212] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0213] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0214] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0215] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0216] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0217] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0218] Example 3

[0219] The rest is the same as in Example 1, except that:

[0220] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0221] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 50° C. for 10 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0222] The dosage ratio of the spherical alumina, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:5.5g:80mL.

[0223] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0224] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0225] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 6.5 g: 100 mL: 0.025 mol: 200 mL.

[0226] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0227] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 60°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and vacuum dried at 80°C for 4 hours to obtain intermediate product III;

[0228] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0229] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0230] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0231] The amount of dibutyltin dilaurate A used is 1.0wt% of the total mass of the reactants.

[0232] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm-1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0233] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing toluene-2,4-diisocyanate and dibutyltin dilaurate B through a peristaltic pump, stirring at 40°C for 10 hours. After the reaction is completed, vacuum distillation is performed, and vacuum drying is performed at 60°C for 8 hours to obtain the intermediate product IV;

[0234] The intermediate product III and toluene-2,4-diisocyanate are added at a molar ratio of hydroxyl group to isocyanate group of 1:2;

[0235] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0236] The usage ratio of toluene-2,4-diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0237] The amount of dibutyltin dilaurate B used is 1.0 wt% of the total mass of the reactants.

[0238] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0239] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 60 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0240] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0241] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0242] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0243] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0244] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0245] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0246] Example 4

[0247] The rest is the same as in Example 1, except that:

[0248] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0249] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0250] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0251] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm-1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0252] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing, and then adding the intermediate product I to N,N-dimethylformamide B containing isophorone diisocyanate by a peristaltic pump, stirring at room temperature for 4 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0253] The usage ratio of the intermediate product I, N,N-dimethylformamide A, isophorone diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0254] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0255] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 120°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and dried in vacuum at 80°C for 4 hours to obtain intermediate product III;

[0256] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0257] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0258] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0259] The amount of dibutyltin dilaurate A used is 1.5wt% of the total mass of the reactants.

[0260] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0261] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing isophorone diisocyanate and dibutyltin dilaurate B by a peristaltic pump, stirring at 100°C for 8 hours. After the reaction is completed, vacuum distillation is performed, and vacuum drying is performed at 60°C for 8 hours to obtain the intermediate product IV;

[0262] The intermediate product III and isophorone diisocyanate are added at a molar ratio of hydroxyl group to isocyanate group of 1:2;

[0263] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0264] The usage ratio of isophorone diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0265] The amount of dibutyltin dilaurate B used is 1.5wt% of the total mass of the reactants.

[0266] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0267] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 120 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0268] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0269] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0270] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0271] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0272] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0273] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0274] Example 5

[0275] The rest is the same as in Example 1, except that:

[0276] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0277] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0278] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0279] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0280] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring to disperse, and then adding the mixture dropwise to N,N-dimethylformamide B containing L-lysine diisocyanate through a peristaltic pump, stirring at room temperature for 4 hours, and after the reaction is completed, performing reduced pressure distillation, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0281] The usage ratio of the intermediate product I, N,N-dimethylformamide A, L-lysine diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0282] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0283] (3) N2 protection, add intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stir, and add dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, react at 100°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, concentrate the solution, distill under reduced pressure, and vacuum dry at 80°C for 4 hours to obtain intermediate product III;

[0284] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0285] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0286] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0287] The amount of dibutyltin dilaurate A used is 1.5wt% of the total mass of the reactants.

[0288] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0289] (4) N2 protection, add the intermediate product III to N,N-dimethylformamide E, stir, and add dropwise to N,N-dimethylformamide F containing L-lysine diisocyanate and dibutyltin dilaurate B through a peristaltic pump, stir at 80°C for 12 hours, and after the reaction is completed, distill under reduced pressure and dry under vacuum at 60°C for 8 hours to obtain the intermediate product IV;

[0290] The intermediate product III and L-lysine diisocyanate are added at a molar ratio of hydroxyl to isocyanate of 1:2;

[0291] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0292] The usage ratio of L-lysine diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0293] The amount of dibutyltin dilaurate B used is 1.5wt% of the total mass of the reactants.

[0294] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm-1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0295] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 100 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0296] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0297] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0298] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0299] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0300] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0301] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0302] Example 6

[0303] The rest is the same as in Example 1, except that:

[0304] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0305] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0306] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0307] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0308] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0309] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0310] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0311] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 60°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and vacuum dried at 80°C for 4 hours to obtain intermediate product III;

[0312] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0313] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0314] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0315] The amount of dibutyltin dilaurate A used is 1.0wt% of the total mass of the reactants.

[0316] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0317] (4) N2 protection, adding the intermediate product III to N,N-dimethylformamide E, stirring, and adding dropwise to N,N-dimethylformamide F containing isophorone diisocyanate and dibutyltin dilaurate B by a peristaltic pump, stirring at 100°C for 8 hours. After the reaction is completed, vacuum distillation is performed, and vacuum drying is performed at 60°C for 8 hours to obtain the intermediate product IV;

[0318] The intermediate product III and isophorone diisocyanate are added at a molar ratio of hydroxyl group to isocyanate group of 1:2;

[0319] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0320] The usage ratio of isophorone diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0321] The amount of dibutyltin dilaurate B used is 1.5wt% of the total mass of the reactants.

[0322] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0323] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 120 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0324] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0325] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0326] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0327] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0328] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0329] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1:-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0330] Example 7

[0331] The rest is the same as in Example 1, except that:

[0332] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0333] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0334] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0335] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0336] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0337] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0338] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm-1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0339] (3) N2 protection, adding intermediate product II and dibutyltin dilaurate A to N,N-dimethylformamide C, stirring, and adding dropwise to N,N-dimethylformamide D containing PPG800 by a peristaltic pump, reacting at 60°C, and the reaction end point is determined by the result of infrared detection of isocyanate; after the reaction, the solution is concentrated, distilled under reduced pressure, and vacuum dried at 80°C for 4 hours to obtain intermediate product III;

[0340] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:2;

[0341] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 200 mL;

[0342] The dosage ratio of PPG800 and N,N-dimethylformamide D is: 10g:150mL;

[0343] The amount of dibutyltin dilaurate A used is 1.0wt% of the total mass of the reactants.

[0344] Its infrared data is as follows: 3445cm -1 :-OH exists and is enhanced; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0345] (4) N2 protection, add the intermediate product III to N,N-dimethylformamide E, stir, and add dropwise to N,N-dimethylformamide F containing L-lysine diisocyanate and dibutyltin dilaurate B through a peristaltic pump, stir at 80°C for 12 hours, and after the reaction is completed, distill under reduced pressure and dry under vacuum at 60°C for 8 hours to obtain the intermediate product IV;

[0346] The intermediate product III and L-lysine diisocyanate are added at a molar ratio of hydroxyl to isocyanate of 1:2;

[0347] The usage ratio of the intermediate product III to N,N-dimethylformamide E is 10 g:200 mL;

[0348] The usage ratio of L-lysine diisocyanate to N,N-dimethylformamide F is 5g:200mL;

[0349] The amount of dibutyltin dilaurate B used is 1.5wt% of the total mass of the reactants.

[0350] Its infrared data is as follows: 3445cm -1 :-OH exists and weakens; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0351] (5) Add graphene oxide to N,N-dimethylformamide G, ultrasonicate for 2 h at 200 W ultrasonic power, add intermediate product IV and dibutyltin dilaurate C, heat to 100 ° C, and determine the reaction end point by infrared detection of isocyanate; after the reaction, filter and rinse with dichloromethane, and place the filter cake in a vacuum dryer at 40 ° C for 24 h to obtain the target product, i.e., modified thermal conductive filler I;

[0352] The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:1.

[0353] The usage ratio of the graphene oxide, N,N-dimethylformamide G, and dichloromethane is 1.0 g: 200 mL: 400 mL;

[0354] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0355] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0356] The amount of dibutyltin dilaurate C used is 0.5wt% of the total mass of the reactants.

[0357] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1:-C=O exists and is enhanced; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist; 1724cm -1 :-C=O (carboxyl) exists (weak peak); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0358] Example 8

[0359] The rest is the same as Example 1, except that the magnesium oxide whiskers are replaced with needle-shaped aluminum oxide.

[0360] Example 9

[0361] The rest is the same as in Example 1, except that:

[0362] A method for preparing a modified thermally conductive filler II comprises the following steps:

[0363] (1) Add magnesium oxide whiskers and mercaptosilane coupling agent KH580 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 50° C. for 10 h, filter, take the insoluble matter, and dry at 60° C. for 12 h to obtain intermediate 1;

[0364] The dosage ratio of the magnesium oxide whisker, the mercaptosilane coupling agent KH580, and the anhydrous ethanol is 1 g:5.5 g:80 mL.

[0365] Its infrared data is as follows: 3438cm -1 :-OH weakened; 2550cm -1 :-SH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0366] (2) N2 protection, the intermediate product 1 is dispersed in N,N-dimethylformamide H, and added dropwise to toluene containing vinyl silicone oil via a peristaltic pump, and the temperature is raised to 30°C and stirred for 4 hours; and then the intermediate product 2 is obtained by vacuum distillation and vacuum drying at 40°C for 24 hours;

[0367] The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group.

[0368] The usage ratio of the intermediate product 1 to N,N-dimethylformamide H is 10 g:200 mL;

[0369] The usage ratio of the vinyl silicone oil to toluene is 10g:150mL.

[0370] Its infrared data is as follows: 3438cm -1 :-OH exists; 2550cm -1 :-SH does not exist; 1625cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0371] (3) The intermediate product 2 was added to tetrahydrofuran, and then added dropwise to toluene containing hydrogenated silicone oil and catalyst chloroplatinic acid via a peristaltic pump, and stirred. After reacting at 70° C. for 5 h, the solvent was removed by vacuum distillation, and the mixture was dried at 80° C. for 4 h to obtain the target product, i.e., the modified thermal conductive filler II;

[0372] The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of 1:2 between vinyl and silicon hydrogen;

[0373] The usage ratio of the intermediate product 2 to tetrahydrofuran is 10 g:200 mL;

[0374] The usage ratio of the hydrogen-containing silicone oil to toluene is 10 g:300 mL;

[0375] The amount of chloroplatinic acid used is 0.05wt% of the total mass of the reactants.

[0376] Its infrared data is as follows: 3438cm -1 :-OH exists; 2150cm -1 :-Si-H exists; 1625cm -1 :-C=C- does not exist; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0377] Example 10

[0378] The rest is the same as in Example 1, except that:

[0379] A method for preparing a modified thermally conductive filler II comprises the following steps:

[0380] (1) Add magnesium oxide whiskers and mercaptosilane coupling agent KH580 to anhydrous ethanol, ultrasonically vibrate for 0.5 h, stand at room temperature for 2 h, react at 80° C. for 4 h, filter, take the insoluble matter, and dry at 60° C. for 12 h to obtain intermediate 1;

[0381] The dosage ratio of the magnesium oxide whisker, the mercaptosilane coupling agent KH580, and the anhydrous ethanol is 1 g:3.5 g:80 mL.

[0382] Its infrared data is as follows: 3438cm -1 :-OH weakened; 2550cm -1 :-SH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0383] (2) N2 protection, the intermediate product 1 is dispersed in N,N-dimethylformamide H, and added dropwise to toluene containing vinyl silicone oil via a peristaltic pump, and the temperature is raised to 50°C and stirred for 2 hours; and then the intermediate product 2 is obtained by vacuum distillation and vacuum drying at 40°C for 24 hours;

[0384] The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group.

[0385] The usage ratio of the intermediate product 1 to N,N-dimethylformamide H is 10 g:200 mL;

[0386] The usage ratio of the vinyl silicone oil to toluene is 10g:150mL.

[0387] Its infrared data is as follows: 3438cm -1 :-OH exists; 2550cm -1 :-SH does not exist; 1625cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0388] (3) The intermediate product 2 is added to tetrahydrofuran, and then added dropwise to toluene containing hydrogenated silicone oil and catalyst chloroplatinic acid via a peristaltic pump, and stirred. After reacting at 120° C. for 4 h, the solvent is removed by vacuum distillation, and the mixture is dried at 80° C. for 4 h to obtain the target product, i.e., the modified thermal conductive filler II;

[0389] The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of 1:2 between vinyl and silicon hydrogen;

[0390] The usage ratio of the intermediate product 2 to tetrahydrofuran is 10 g:200 mL;

[0391] The usage ratio of the hydrogen-containing silicone oil to toluene is 10 g:300 mL;

[0392] The amount of chloroplatinic acid used is 0.05wt% of the total mass of the reactants.

[0393] Its infrared data is as follows: 3438cm -1 :-OH exists; 2150cm -1 :-Si-H exists; 1625cm -1 :-C=C- does not exist; 1109cm -1 、801cm -1 :-Si-O- exists; 599cm -1 :-Mg-O- exists.

[0394] Embodiment 11

[0395] The rest is the same as in Example 1, except that:

[0396] A thermal conductive coating comprises the following raw materials in parts by weight:

[0397] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0398] 8.16 parts of modified thermally conductive filler I;

[0399] Modified thermal conductive filler II 2.04 parts;

[0400] TPGDA 4.0 copies;

[0401] PO-TMPTA 4.0 parts;

[0402] PETTA 2.0 parts;

[0403] 3.0 parts of photoinitiator;

[0404] Leveling agent 401LS 0.3 parts;

[0405] Residue of organic solvent;

[0406] The total amount of the above components is 100 parts.

[0407] Example 12

[0408] The rest is the same as in Example 1, except that:

[0409] A thermal conductive coating comprises the following raw materials in parts by weight:

[0410] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0411] 7.65 parts of modified thermally conductive filler I;

[0412] 2.55 parts of modified thermal conductive filler II;

[0413] TPGDA 4.0 copies;

[0414] PO-TMPTA 4.0 parts;

[0415] PETTA 2.0 parts;

[0416] 3.0 parts of photoinitiator;

[0417] Leveling agent 401LS 0.3 parts;

[0418] Residue of organic solvent;

[0419] The total amount of the above components is 100 parts.

[0420] Embodiment 13

[0421] The rest is the same as in Example 1, except that:

[0422] A thermal conductive coating comprises the following raw materials in parts by weight:

[0423] 40.0 parts of polyurethane acrylate prepolymer (Sartomer CN965 and Cytec EB205H mixed in a mass ratio of 1 / 2);

[0424] 5.4 parts of modified thermally conductive filler I;

[0425] 1.5 parts of modified thermal conductive filler II;

[0426] TPGDA 3.0 copies;

[0427] PO-TMPTA 4.0 parts;

[0428] PETTA 1.0 part;

[0429] 3.0 parts of photoinitiator;

[0430] Leveling agent 401LS 0.3 parts;

[0431] Residue of organic solvent;

[0432] The total amount of the above components is 100 parts.

[0433] Embodiment 14

[0434] The rest is the same as in Example 1, except that:

[0435] A thermal conductive coating comprises the following raw materials in parts by weight:

[0436] 60.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0437] Modified thermal conductive filler I 10.0 parts;

[0438] Modified thermal conductive filler II 2.8 parts;

[0439] TPGDA 6.0 copies;

[0440] PO-TMPTA 6.0 parts;

[0441] PETTA 3.0 parts;

[0442] 3.0 parts of photoinitiator;

[0443] Leveling agent 401LS 0.3 parts;

[0444] Residue of organic solvent;

[0445] The total amount of the above components is 100 parts.

[0446] Embodiment 15

[0447] The rest is the same as in Example 1, except that:

[0448] A thermal conductive coating comprises the following raw materials in parts by weight:

[0449] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0450] 8.0 parts of modified thermally conductive filler I;

[0451] Modified thermal conductive filler II 2.2 parts;

[0452] TPGDA 4.0 copies;

[0453] PO-TMPTA 4.0 parts;

[0454] PETTA 2.0 parts;

[0455] Photoinitiator 5.0 parts;

[0456] Leveling agent 401LS 0.1 part;

[0457] Residue of organic solvent;

[0458] The total amount of the above components is 100 parts.

[0459] A method for preparing a glue-filled power supply housing comprises the following steps:

[0460] The thermal conductive coating was evenly coated on the substrate under N2 protection, heated at 80°C for 180s, and the coating layer was irradiated with UV light at an irradiation energy of 400mJ / cm 2 , the irradiation time is 60s, and the glue-filled power supply shell with a dry film thickness of 40μm is obtained.

[0461] Example 16

[0462] The rest is the same as in Example 1, except that:

[0463] A thermal conductive coating comprises the following raw materials in parts by weight:

[0464] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0465] 8.0 parts of modified thermally conductive filler I;

[0466] Modified thermal conductive filler II 2.2 parts;

[0467] TPGDA 4.0 copies;

[0468] PO-TMPTA 4.0 parts;

[0469] PETTA 2.0 parts;

[0470] 2.0 parts of photoinitiator;

[0471] Leveling agent 401LS 0.4 parts;

[0472] Residue of organic solvent;

[0473] The total amount of the above components is 100 parts.

[0474] A method for preparing a glue-filled power supply housing comprises the following steps:

[0475] Under N2 protection, the thermal conductive coating was evenly coated on the substrate, heated at 80°C for 180s, and the coating layer was irradiated with UV light at an irradiation energy of 600mJ / cm 2 , the irradiation time is 30s, and the glue-filled power supply shell with a dry film thickness of 30μm is obtained.

[0476] The following comparative examples are compared with specific embodiment 1:

[0477] Comparative Example 1

[0478] The rest is the same as in Example 1, except that:

[0479] A thermal conductive coating comprises the following raw materials in parts by weight:

[0480] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0481] TPGDA 4.0 copies;

[0482] PO-TMPTA 4.0 parts;

[0483] PETTA 2.0 parts;

[0484] 3.0 parts of photoinitiator;

[0485] Leveling agent 401LS 0.3 parts;

[0486] Residue of organic solvent;

[0487] The total amount of the above components is 100 parts.

[0488] Comparative Example 2

[0489] The rest is the same as in Example 1, except that:

[0490] A thermal conductive coating comprises the following raw materials in parts by weight:

[0491] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0492] 10.2 parts of modified thermal conductive filler II;

[0493] TPGDA 4.0 copies;

[0494] PO-TMPTA 4.0 parts;

[0495] PETTA 2.0 parts;

[0496] 3.0 parts of photoinitiator;

[0497] Leveling agent 401LS 0.3 parts;

[0498] Residue of organic solvent;

[0499] The total amount of the above components is 100 parts.

[0500] Comparative Example 3

[0501] The rest is the same as in Example 1, except that:

[0502] A thermal conductive coating comprises the following raw materials in parts by weight:

[0503] 50.0 parts of polyurethane acrylate prepolymer (mixed with Sartomer CN965 and Cytec EB205H in a mass ratio of 1 / 2);

[0504] Modified thermal conductive filler I10.2 parts;

[0505] TPGDA 4.0 copies;

[0506] PO-TMPTA 4.0 parts;

[0507] PETTA 2.0 parts;

[0508] 3.0 parts of photoinitiator;

[0509] Leveling agent 401LS 0.3 parts;

[0510] Residue of organic solvent;

[0511] The total amount of the above components is 100 parts.

[0512] Comparative Example 4

[0513] The rest is the same as in Example 1, except that:

[0514] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0515] (1) Spherical alumina and aminosilane coupling agent KH550 were added to anhydrous ethanol, ultrasonically vibrated for 0.5 h, allowed to stand at room temperature for 2 h, reacted at 60° C. for 5 h, filtered, the insoluble matter was taken, and dried at 60° C. for 12 h to obtain intermediate product I;

[0516] The usage ratio of the spherical alumina, the aminosilane coupling agent KH550 and the anhydrous ethanol is 1g:4.5g:80mL.

[0517] Its infrared data is as follows: 3438cm -1 :-OH weakened; 1560cm -1 : -NH sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists.

[0518] (2) adding the intermediate product I to N,N-dimethylformamide A and stirring and dispersing it, and then adding it dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate through a peristaltic pump, stirring at room temperature for 2 hours, and after the reaction is completed, distilling under reduced pressure, and vacuum drying at 60° C. for 8 hours to obtain the intermediate product II;

[0519] The usage ratio of the intermediate product I, N,N-dimethylformamide A, toluene-2,4-diisocyanate, and N,N-dimethylformamide B is: 5.4 g: 100 mL: 0.02 mol: 200 mL.

[0520] Its infrared data is as follows: 3438cm -1 :-OH exists; 2928cm -1 :-CH exists; 1719cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO exists.

[0521] (3) N2 protection, adding intermediate II, dibutyltin dilaurate, and PPG800 to N,N-dimethylformamide C, stirring, and reacting at 60°C. The reaction end point is determined by the result of infrared detection of isocyanate. After the reaction, the solution is concentrated, distilled under reduced pressure, and dried in vacuum at 80°C for 4 hours to obtain the target product.

[0522] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:1;

[0523] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 300 mL;

[0524] The amount of dibutyltin dilaurate used is 1.0wt% of the total mass of the reactants.

[0525] Its infrared data is as follows: 3445cm -1 :-OH exists; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1560cm -1 :-NH exists; 1109cm -1 、801cm -1 :-Si-O- exists; 607cm -1 、771cm -1 :-Al-O- exists; 2270cm -1 :-NCO does not exist.

[0526] Comparative Example 5

[0527] The rest is the same as in Example 1, except that:

[0528] A method for preparing a modified thermally conductive filler I comprises the following steps:

[0529] (1) Graphene oxide was added to N,N-dimethylformamide A, and after ultrasonication at 200 W for 2 h, the mixture was added dropwise to N,N-dimethylformamide B containing toluene-2,4-diisocyanate and dibutyltin dilaurate A through a peristaltic pump, and stirred at 40° C. for 10 h. After the reaction was completed, the mixture was distilled under reduced pressure, and vacuum dried at 40° C. for 12 h to obtain an intermediate product I;

[0530] The toluene-2,4-diisocyanate and graphene oxide are added at a molar ratio of isocyanate to hydroxyl of 2:1.

[0531] The usage ratio of graphene oxide and N,N-dimethylformamide A is 1.0 g: 200 mL;

[0532] The hydroxyl content of the graphene oxide is 5 mmol / g;

[0533] The graphene oxide is graphene oxide prepared by improving Hummer's method;

[0534] The amount of dibutyltin dilaurate A used is 1.5wt% of the total mass of the reactants.

[0535] Its infrared data are as follows: 3440cm -1 :-OH does not exist; 2270cm -1 :-NCO exists; 2953cm -1 :-CH exists; 1724cm -1 :-C=O exists; 1734cm -1 :-C=O exists (weak peak of carboxyl group); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0536] (2) N2 protection, adding the intermediate product I, dibutyltin dilaurate, and PPG800 to N,N-dimethylformamide C, stirring, and reacting at 60°C. The reaction end point is determined by the result of infrared detection of isocyanate. After the reaction, the solution is concentrated, distilled under reduced pressure, and dried in vacuum at 80°C for 4 hours to obtain the target product.

[0537] The intermediate product II and PPG800 are added at a molar ratio of isocyanate to hydroxyl of 1:1;

[0538] The usage ratio of the intermediate product II and N,N-dimethylformamide C is: 10 g: 300 mL;

[0539] The amount of dibutyltin dilaurate used is 1.0wt% of the total mass of the reactants.

[0540] Its infrared data is as follows: 3445cm -1 :-OH does not exist; 2928cm -1 :-CH exists; 1724cm -1 :-C=O exists and is enhanced; 2270cm -1 :-NCO does not exist; 1734cm -1 :-C=O exists (weak peak of carboxyl group); 1218cm -1 、1104cm -1 : Epoxy group exists (weak peak).

[0541] Comparative Example 6

[0542] The rest is the same as in Example 1, except that PPG800 is replaced by PPG200.

[0543] Comparative Example 7

[0544] The rest is the same as in Example 1, except that:

[0545] The magnesium oxide whiskers were replaced with nano magnesium oxide with an average particle size of 100 nm.

[0546] Comparative Example 8

[0547] The rest is the same as in Example 1, except that:

[0548] A preparation method of a modified thermally conductive filler II is the same as that of the modified thermally conductive filler I in comparative example 4, except that the spherical aluminum oxide is replaced with magnesium oxide whiskers.

[0549] Comparative Example 9

[0550] The rest is the same as in Example 1, except that:

[0551] The difference is that the polyurethane acrylate prepolymer is replaced by an epoxy acrylate prepolymer (Sartomer CN151 and Changxing 6261 are mixed in a mass ratio of 1 / 2).

[0552] Comparative Example 10

[0553] Prepared directly from substrate without thermal conductive coating.

[0554] The physical properties of the thermal conductive coatings of the glue-filled power supply shells prepared in Examples 1-16 of the present invention and Comparative Examples 1-10 were measured respectively, and the results are shown in Table 1.

[0555] Table 1 Physical test performance of each embodiment

[0556]

[0557]

[0558] First, compared with comparative examples 1-10, examples 1-16 show that the thermal conductive coating of the present invention has excellent adhesion and bonding strength, and also has excellent flexibility.

[0559] Second, it can be observed from Example 1 and Comparative Examples 1-3 that the modified thermally conductive filler I and modified thermally conductive filler II of the present invention have excellent thermal conductivity; it can be observed from Example 1 and Comparative Examples 4-6 that the spherical oxides and graphene in the modified thermally conductive filler I have a synergistic effect on thermal conductivity; in addition, different soft segment diols have a greater influence on the flexibility of the coating; it can be observed from Example 1 and Comparative Examples 7-8 that the needle-shaped or whisker oxides in the modified thermally conductive filler II have an important influence on the final network stereo maximization of thermal conductivity; in addition, the residual silicon hydrogen structure has a positive effect on the improvement of the adhesion of the sealant; it can be observed from Example 1 and Comparative Example 9 that the polyurethane modified acrylate system has better flexibility than the epoxy modified acrylate system; it can be observed from Example 1 and Comparative Example 10 that the thermally conductive coating of the present invention has excellent thermal conductivity and can effectively improve the adhesion between the sealant and the substrate.

[0560] In summary, modified thermal conductive filler I and modified thermal conductive filler II have excellent flexibility, adhesion and thermal conductivity in the polyurethane system, and can be used as an effective transition coating between the sealant and the substrate, which has great practical significance.

[0561] The test method is as follows:

[0562] (1) Adhesion: The adhesion test was performed according to the method described in ASTM D3359-17.

[0563] (2) Bonding strength: The method described in GB / T13936-2014 was followed. The potting compound used was a two-component addition-type silicone compound, model KE-1184-AB, Shin-Etsu, Japan. The bonding strength of the potting compound to the coating was tested.

[0564] (3) Flexibility: tested according to the method described in GB / T 1731-2020.

[0565] (4) Thermal conductivity: Tested according to the method described in ASTM E1461.

[0566] (5) Hot and cold cycle test: The sample to be tested (power supply containing potting glue, potting glue is KE-1184-AB, Shin-Etsu, Japan) is placed at -40℃ and +85℃ for testing, and each temperature is placed for 24 hours. After 1000 cycles, observe whether there is delamination between the sealant and the coating.

[0567] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A glue-filled power supply shell, Features: It comprises a power supply housing, the inner surface of which is coated with a thermal conductive coating; The thermal conductive coating comprises the following raw materials in parts by weight: 40.0-60.0 parts of polyurethane acrylate prepolymer; Modified thermally conductive filler I 5.0-10.0 parts; Modified thermal conductive filler II 1.5-3.0 parts; UV monomer diluent 8.0-15.0 parts; Photoinitiator 2.0-5.0 parts; Leveling agent 0.1-0.4 parts; Residue of organic solvent; The total amount of the above components is 100 parts; The preparation method of the modified thermally conductive filler I comprises the following steps: (1) Metal oxide A and aminosilane coupling agent are placed in an alcohol solvent to carry out silylation coupling reaction to prepare intermediate product I; (2) The intermediate product I undergoes a condensation reaction with an asymmetric diisocyanate A to prepare an intermediate product II; (3) The intermediate product II is subjected to a condensation reaction with a diol in the presence of a catalyst, dibutyltin dilaurate A, to prepare an intermediate product III; (4) The intermediate product III is subjected to a condensation reaction with an asymmetric diisocyanate B in the presence of a catalyst, dibutyltin dilaurate B, to prepare an intermediate product IV; (5) The intermediate product IV undergoes a condensation reaction with graphene oxide under the action of a catalyst, dibutyltin dilaurate C, to obtain a target product, i.e., a modified thermal conductive filler I; The preparation method of the modified thermally conductive filler II comprises the following steps: (1) Metal oxide B and mercaptosilane coupling agent are placed in an alcohol solvent to carry out silylation coupling reaction to prepare intermediate product 1; (2) Intermediate product 1 undergoes a "thiol-ene" click reaction with vinyl silicone oil to prepare intermediate product 2; (3) The intermediate product 2 is subjected to a hydrosilylation reaction with hydrogen-containing silicone oil in the presence of a catalyst, chloroplatinic acid, to obtain the target product, i.e., the modified thermal conductive filler II; The metal oxide A is a spherical structure; The metal oxide B is in a needle-like or whisker structure.

2. The glue-filled power supply housing according to claim 1, Features: The modified thermally conductive filler I and the modified thermally conductive filler II are mixed at a mass ratio of 3.0-4.0:

1.

3. The glue-filled power supply housing according to claim 1, Features: In step (1) of the preparation method of the modified thermally conductive filler I, the amount of the metal oxide A, the aminosilane coupling agent, and the alcohol solvent is 1 g: 3.3-5.5 g: 80 mL; The usage ratio of the intermediate product I and the asymmetric diisocyanate A is 4.3-6.5 g: 0.015-0.025 mol; The diol is a polyether diol or a polyester diol; The intermediate product II and the diol are added in a molar ratio of isocyanate to hydroxyl of 1:2; The amount of dibutyltin dilaurate A is 1.0-1.5wt% of the total mass of the reactants; The intermediate product III and the asymmetric diisocyanate B are added at a molar ratio of hydroxyl to isocyanate of 1:2; The amount of dibutyltin dilaurate B is 1.0-1.5wt% of the total mass of the reactants; The hydroxyl content of the graphene oxide is 5 mmol / g; The graphene oxide is graphene oxide prepared by improving Hummer's method; and The intermediate product IV and graphene oxide are added in a molar ratio of isocyanate to hydroxyl of 1:

1.

4. The glue-filled power supply housing according to claim 1, Features: In step (1) of the preparation method of the modified thermally conductive filler II, the amount of the metal oxide B, the mercaptosilane coupling agent, and the alcohol solvent is 1 g: 3.3-5.5 g: 80 mL; The intermediate product 1 and the vinyl silicone oil are added in a ratio of 1:2 between the mercapto group and the vinyl group; and The intermediate product 2 and the hydrogen-containing silicone oil are added in a ratio of vinyl to silicon hydrogen of 1:

2.

5. The glue-filled power supply housing according to claim 1, Features: The preparation method of the thermal conductive coating is as follows: Protect from light, keep humidity ≤60%, mix the leveling agent and organic solvent evenly to obtain a mixed solvent, add polyurethane acrylate prepolymer, UV monomer diluent, modified thermal conductive filler I and modified thermal conductive filler II to the mixed solvent in sequence, continue to stir evenly, add photoinitiator, stir evenly, filter with filter cloth with a pore size of 1 μm, and obtain the thermal conductive coating.

6. The method for preparing the glue-filled power supply housing according to any one of claims 1 to 5, Features: The steps include: The thermal conductive coating is evenly coated on the inner surface of the power supply housing, the solvent is removed by heating, and the coating layer is subjected to UV irradiation to obtain a glue-filled power supply housing.