A method for preparing vinyl sulfate using a continuous flow reaction system
By using a combination of a continuous flow reaction system and a TiO2 or CeO2 support composite catalyst in the preparation of vinyl sulfate, the problem of insufficient operability and safety in traditional processes is solved, and efficient and economical preparation of vinyl sulfate and large-scale production of vinyl sulfate is achieved. Continuous automated production.
Patent Information
- Application Number
- CN202410341607.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-25
AI Technical Summary
The traditional kettle process has low operability and safety when preparing vinyl sulfate, and the reaction is not carried out at a high level, making it difficult to achieve large-scale continuous automated production.
A continuous flow reaction system is used to combine TiO2 or CeO2 as a support composite catalyst to prepare vinyl sulfate through cyclization, neutralization and oxidation reactions, improving the operability and safety of the reaction, and achieving large-scale continuous and automated production.
The yield and reaction efficiency of vinyl sulfate are improved, the economy and environmental protection of the preparation process are ensured, and the composite catalyst can be recycled, extending the service life of the catalyst.
Smart Images

Figure CN118255742B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery electrolyte additives, in particular to a method for preparing vinyl sulfate by using a continuous flow reaction system. Background Art
[0002] At present, energy issues have become the focus of people's attention, and new energy technology is a key development project in various countries. In order to save oil resources and solve pollution problems, new energy vehicles driven by lithium-ion power batteries have become the development direction of the new energy vehicle industry. DTD chemical substance, Chinese name Ethylene sulfate, English name Ethylene sulfate, molecular formula C2H4O4S, is currently an important battery electrolyte additive. The problems of existing new energy vehicle batteries are low cycle times and battery attenuation. The addition of DTD can effectively improve the above problems of electric vehicle batteries, inhibit the initial capacity decline of lithium-ion batteries, high and low temperature performance compatibility, increase initial discharge capacity, extend battery cycle life, and improve battery charge and discharge performance. It is an excellent lithium-ion battery electrolyte additive.
[0003] Existing patent documents report a large number of methods for synthesizing vinyl sulfate, such as: CN109369609A uses a traditional kettle reactor to prepare vinyl sulfate. The scheme is as follows:
[0004] (1) Cyclization reaction: Add 100 g of ethylene glycol and 100 g of dichloromethane to reactor A, adjust the temperature of the reactor to 12°C, dropwise add 250 g of thionyl chloride for 30 min, and continue the reaction for 2 h after the dropwise addition is complete. After the reaction is complete, perform vacuum distillation to remove HCl and unreacted SOCl2, then add saturated sodium bicarbonate aqueous solution for washing until the pH value of the solution is ≥7, perform liquid separation, and obtain 210 g of dichloromethane solution of vinyl sulfite, containing 152 g of product, with a yield of 87.3%. Transfer the dichloromethane solution of vinyl sulfite to reactor B for standby use.
[0005] (2) Oxidation reaction: 100 g of dichloromethane and 0.69 g of 10% potassium dihydrogen phosphate solution were added to the reactor B, and the pH was adjusted to 9 with 15% sodium bicarbonate solution. The temperature of the reactor was lowered to 8°C, and 697.7 g of 30% sodium hypochlorite aqueous solution was added dropwise for 1 hour. After the sodium hypochlorite was added dropwise, the reaction was continued for 3 hours to obtain a dichloromethane solution of vinyl sulfate. The reaction solution was allowed to stand and separated to obtain a dichloromethane solution. The aqueous phase was extracted twice with dichloromethane, and the dichloromethane solutions were combined.
[0006] (3) The mixture was concentrated under reduced pressure at 10° C. until a white solid appeared. 300 g of n-hexane was added for recrystallization. The mixture was filtered to obtain 108.1 g of vinyl sulfate with a yield of 61.9%, a purity of 99.93%, a moisture content of 34 ppm, and an acid value of 27 ppm.
[0007] In patent CN109369609A, the traditional kettle process is used to prepare vinyl sulfate. Compared with the continuous flow reaction, the traditional kettle process has lower operability and safety, and its reaction rate is not as high as that of the continuous flow reaction. Summary of the invention
[0008] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing vinyl sulfate using a continuous flow reaction system. The continuous flow reaction system combined with the composite catalyst provided by the present invention can improve the operability and safety of the reaction, while realizing large-scale continuous automated production and improving the efficiency of the reaction. The composite catalyst uses TiO2 or CeO2 as a carrier, and the vinyl sulfate prepared therefrom has a high yield, is economical and environmentally friendly, and can be recycled.
[0009] The present invention provides a method for preparing vinyl sulfate using a continuous flow reaction system, comprising the following steps:
[0010] Ethylene glycol, thionyl chloride, ammonia water, an oxidant and a composite catalyst are sequentially subjected to cyclization, neutralization and oxidation reactions in a continuous flow reaction system to obtain vinyl sulfate;
[0011] The composite catalyst comprises a carrier and ruthenium trichloride loaded on the carrier; the carrier is TiO2 or CeO2.
[0012] The continuous flow reaction system of the present invention comprises a continuous flow reactor A and a continuous flow reactor B, and the continuous flow reactor A and the continuous flow reactor B comprise a heat exchange layer and a reaction layer. The number of parallel connection of the continuous flow reaction system of the present invention is one or more, and multiple parallel production can achieve production expansion. In certain technical schemes of the present invention, the number of parallel connection of the continuous flow reaction system of the present invention is 1 to 8. The continuous flow reaction system of the present invention enables the reaction materials to pass continuously in the continuous flow reactor; the function of the heat exchange layer is heat exchange, and heat exchange refers to the heat exchange of the thermal effect generated by the continuous flow reaction, including the heat exchange of the material in the continuous flow reactor module; the material is transported by a peristaltic pump. The continuous flow reaction system of the present invention can improve the operability and safety of the reaction, while realizing large-scale continuous automated production and improving the efficiency of the reaction.
[0013] The composite catalyst of the present invention is a heterogeneous composite catalyst. Heterogeneous catalysis is also called multiphase catalysis or contact catalysis, which refers to the catalytic reaction caused by the catalyst and the reactant being in different phases on the catalyst interface. The carrier in the composite catalyst of the present invention is TiO2 or CeO2, preferably TiO2. In one technical solution of the present invention, the carrier is selected from P25, and P25 refers to titanium dioxide in a mixed phase of anatase crystal and rutile crystal with an average particle size of 25nm. In some technical solutions of the present invention, the mass ratio of ruthenium in ruthenium trichloride in the composite catalyst to the carrier is (0.0005-0.0015):1. In one technical solution of the present invention, the mass ratio of ruthenium in ruthenium trichloride in the composite catalyst to the carrier is 0.000579:1. In another technical solution of the present invention, the mass ratio of ruthenium in ruthenium trichloride in the composite catalyst to the carrier is 0.00125:1.
[0014] The inventors of the present application creatively discovered that by selecting TiO2 or CeO2 as a carrier and loading ruthenium trichloride on the carrier, the resulting composite catalyst can be used for the preparation of vinyl sulfate, which can greatly improve the yield of vinyl sulfate, and the catalytic effect of the composite catalyst is less reduced after being recycled multiple times; at the same time, the composite catalyst is used in a continuous flow reaction system to prepare vinyl sulfate, which can improve the operability and safety of the reaction, while improving the efficiency of the reaction.
[0015] The temperature of the oxidation reaction of the present invention is 0-10° C., preferably 0-5° C. The oxidation reaction of the present invention is specifically to mix the product after the neutralization reaction with the oxidant and the composite catalyst in a continuous flow reaction system and perform the oxidation reaction at a temperature of 0-5° C.; more specifically, the product after the neutralization reaction and the oxidant are mixed and then flowed into a continuous flow reaction system containing a composite catalyst and perform the oxidation reaction at a temperature of 0-5° C.
[0016] The oxidation reaction of the present invention can be continuously carried out in a continuous flow reaction system by controlling the flow rate of each material according to the concentration and dosage ratio of each material. In each continuous flow reaction system, the dosage ratio of ethylene glycol, thionyl chloride, ammonia water, oxidant and composite catalyst of the present invention every 2 to 4 hours is 4 mol: (4 to 4.2) mol: (8.03 to 8.99) mol: 4.02 mol: (400 to 1200) g, preferably 4 mol: (4 to 4.2) mol: (8.03 to 8.99) mol: 4.02 mol: (480 to 1012) g. In certain technical solutions of the present invention, the usage ratio of ethylene glycol, thionyl chloride, ammonia water, oxidant and ruthenium in the composite catalyst every 2 to 4 hours is 4 mol: (4 to 4.2) mol: (8.03 to 8.99) mol: 4.02 mol: (0.00554 to 0.00633) mol, preferably 4 mol: (4 to 4.2) mol: (8.03 to 8.99) mol: 4.02 mol: (0.00554 to 0.00594) mol. The oxidant of the present invention is selected from sodium periodate.
[0017] The composite catalyst is obtained by reacting a carrier, a reducing agent and ruthenium trichloride in water. Specifically, the composite catalyst is obtained by mixing the carrier and ruthenium trichloride in water for more than 10 hours, preferably 10 hours to 24 hours, more preferably 10 hours to 16 hours, and more preferably 12 hours, and then adding a reducing agent thereto for reaction. In certain technical schemes of the present invention, the preparation method of the composite catalyst is: mixing and stirring the carrier, ruthenium trichloride and most of the water for more than 10 hours, preferably 10 hours to 24 hours, more preferably 10 hours to 16 hours, and more preferably 12 hours, and then adding a reducing agent and the remaining water thereto to mix and stir to obtain a composite catalyst; in one technical scheme of the present invention, the volume ratio of the majority of water to the remaining water is 150:1. The usage ratio of the carrier, the reducing agent, the ruthenium trichloride and the water in the present invention is (500-1078) g: 10 g: 1280 mg: 30.2 L. In one technical solution of the present invention, the ratio of the carrier, the reducing agent, ruthenium trichloride and water is 500g:10g:1280mg:30.2L. In another technical solution of the present invention, the ratio of the carrier, the reducing agent, ruthenium trichloride and water is 1078g:10g:1280mg:30.2L. In one technical solution of the present invention, the reducing agent of the present invention is selected from sodium borohydride, the carrier is selected from P25 titanium dioxide, and the mass ratio of sodium borohydride to P25 titanium dioxide is 0.02:1.
[0018] The method for preparing vinyl sulfate using a continuous flow reaction system specifically comprises the following steps:
[0019] Ethylene glycol and thionyl chloride are subjected to a cyclization reaction in a continuous flow reactor A, and then the product obtained by the cyclization reaction is subjected to a neutralization reaction with ammonia water. Then, the product obtained after the neutralization reaction, an oxidant and a composite catalyst are mixed, and then an oxidation reaction is carried out in a continuous flow reactor B to obtain vinyl sulfate.
[0020] The present invention firstly performs a cyclization reaction on ethylene glycol and thionyl chloride in a continuous flow reactor A; specifically, ethylene glycol and thionyl chloride are mixed at a temperature of 0 to 5° C., and the cyclization reaction of the present invention can be continuously performed in the continuous flow reactor A by controlling the flow rate of each material according to the concentration and dosage ratio of each material.
[0021] After the cyclization reaction, the product obtained after the cyclization reaction and ammonia water are subjected to a neutralization reaction, and then the product obtained after the neutralization reaction, an oxidant and the composite catalyst are subjected to an oxidation reaction in a continuous flow reactor B to obtain vinyl sulfate. The specific process is the same as above and will not be repeated.
[0022] The present invention provides a method for preparing vinyl sulfate using a continuous flow reaction system, comprising the following steps: ethylene glycol, thionyl chloride, ammonia water, an oxidant and a composite catalyst are sequentially subjected to cyclization, neutralization and oxidation reactions in a continuous flow reaction system to obtain vinyl sulfate; the composite catalyst comprises a carrier and ruthenium trichloride loaded on the carrier; the carrier is TiO2 or CeO2. The continuous flow reaction system combined with the composite catalyst provided by the present invention is used to prepare vinyl sulfate, which can improve the operability and safety of the reaction, while realizing large-scale continuous automated production and improving the efficiency of the reaction. The composite catalyst uses TiO2 or CeO2 as a carrier, and the vinyl sulfate prepared by the composite catalyst has a high yield, is economical and environmentally friendly, and can be recycled. Experiments show that the composite catalyst of the present invention is used to prepare vinyl sulfate in combination with a continuous flow reaction system, which can be used for large-scale continuous automated production, and the composite catalyst uses TiO2 or CeO2 as a carrier, and the vinyl sulfate prepared by the composite catalyst has a high yield, is economical and environmentally friendly, and can be recycled. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the process for preparing vinyl sulfate in a continuous flow reaction system. DETAILED DESCRIPTION
[0024] The present invention discloses a method for preparing vinyl sulfate using a continuous flow reaction system. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0025] The present invention will be further described below in conjunction with embodiments:
[0026] Example 1
[0027] 1280 mg of ruthenium trichloride and 30 L of water were added to 500 g of titanium dioxide (TiO2), and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 1 was obtained by filtration and washing; the mass ratio of ruthenium in ruthenium trichloride in the heterogeneous composite catalyst 1 to the carrier was 0.00125:1.
[0028] Example 2
[0029] 1280 mg of ruthenium trichloride and 30 L of water were added to 1078 g of cerium oxide (CeO2), and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 4 was obtained by filtration and washing; the mass ratio of ruthenium in ruthenium trichloride in the heterogeneous composite catalyst 2 to the carrier was 0.000579:1.
[0030] Comparative Example 1
[0031] 1280 mg of ruthenium trichloride and 30 L of water were added to 470 g of cobalt oxide (CoO), and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 3 was obtained by filtration and washing; the mass ratio of ruthenium in ruthenium trichloride in the heterogeneous composite catalyst 3 to the carrier was 0.00133:1.
[0032] Comparative Example 2
[0033] 1280 mg of ruthenium trichloride and 30 L of water were added to 544 g of manganese oxide (MnO2), and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 4 was obtained by filtering and washing; the mass ratio of ruthenium in ruthenium trichloride in the heterogeneous composite catalyst 4 to the carrier was 0.00115:1.
[0034] Comparative Example 3
[0035] 1280 mg of ruthenium trichloride and 30 L of water were added to 376 g of silicon dioxide (SiO2), and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 5 was obtained by filtering and washing; the mass ratio of ruthenium in ruthenium trichloride in the heterogeneous composite catalyst 1 to the carrier was 0.00166:1.
[0036] Comparative Example 4
[0037] 1086 mg of palladium dichloride and 30 L of water were added to 500 g of titanium dioxide, and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 6 was obtained by filtering and washing.
[0038] Comparative Example 5
[0039] 824 mg of copper chloride and 30 L of water were added to 500 g of titanium dioxide, and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 7 was obtained by filtering and washing.
[0040] Comparative Example 6
[0041] 776 mg of ferrous chloride and 30 L of water were added to 500 g of titanium dioxide, and the three were mixed and stirred for 12 hours. Then, 10 g of sodium borohydride and 200 mL of water were added and stirred again. The heterogeneous composite catalyst 8 was obtained by filtering and washing.
[0042] Example 3
[0043] The heterogeneous composite catalyst prepared in Example 1 was used to prepare vinyl sulfate in a continuous flow reaction system. The process is as follows: Figure 1 As shown, Figure 1 The schematic diagram of the process of preparing vinyl sulfate in a continuous flow reaction system is as follows:
[0044] Prepare 2L of 2mol / L ethylene glycol in dichloromethane solution, place it in a sealed container and mark it as solution 1; prepare 290mL of dichlorothionyl (4.0mol), place it in a sealed container and mark it as solution 2; prepare 600mL of 25-28wt% ammonia water, place it in a sealed container and mark it as solution 3; prepare 6L of 0.67mol / L sodium periodate solution in water and acetonitrile (the volume ratio of water to acetonitrile is 3:2), place it in a sealed container and mark it as solution 5.
[0045] Solution 1 was cooled to 0°C, and then flowed into mixer A through a pipeline at a flow rate of 1 L / h through peristaltic pump 1. The temperature of mixer A was controlled at 0°C. At the same time, solution 2 was flowed into mixer A through a pipeline at a flow rate of 0.145 L / h through peristaltic pump 2. After mixing with solution 1, it flowed into continuous flow reactor A. The continuous flow reactor was placed at room temperature of 25°C. After solutions 1 and 2 reacted in the continuous flow reactor, the outflow solution was added to solution 3 for neutralization to obtain a mixed solution and marked as solution 4.
[0046] Solution 5 was cooled to 0°C, and then flowed into mixer B through a pipeline at a flow rate of 3L / h through a peristaltic pump 5, and the temperature of mixer B was controlled at 0°C. At the same time, solution 4 was flowed into mixer B through a pipeline at a flow rate of 1.41L / h through a peristaltic pump 4, and after mixing with solution 5, it flowed into a fixed bed continuous flow reactor B containing 468g of the heterogeneous composite catalyst 1 prepared in Example 1 above, and the temperature of continuous flow reactor B was controlled at 0°C. Solutions 4 and 5 were reacted in the continuous flow reactor and then flowed out to obtain a reaction solution. The reaction solution was subjected to extraction, reduced pressure distillation, and recrystallization to obtain 402g of white crystalline vinyl sulfate, with a yield of 81%; purity ≥99.9%; water content ≤50ppm.
[0047] According to the method of this embodiment, the heterogeneous composite catalysts 2 to 8 prepared in Example 2 and Comparative Examples 1 to 6 were respectively used in a continuous flow reaction system to prepare vinyl sulfate, the only difference being the amount of the composite catalyst used.
[0048] The preparation of vinyl sulfate by the above heterogeneous composite catalyst is shown in Table 1:
[0049] Table 1
[0050] Heterogeneous composite catalyst 1 2 3 4 5 6 7 8 Composite catalyst dosage (g) 468 1010 440 510 352 552 728 773 Vinyl sulfate yield% 81 70 35 23 55 15 0 0
[0051] Since the heterogeneous composite catalyst is fixed on a fixed bed, in theory, as long as the catalyst activity does not decrease, the continuous flow reaction can be carried out on the basis of guaranteeing the raw materials. In order to test the service life of the heterogeneous composite catalyst, Example 3 is used as a reaction test. After the reaction is completed, the raw material sample is prepared again and reacted in the continuous flow reactor according to the steps of Example 3. Table 2 is a graph showing the change of the continuous flow reaction test 5 times and the yield. It can be seen from Table 2 that the catalytic effect of the heterogeneous composite catalyst still maintains a high catalytic activity after 5 tests. The time required for each group of tests is 2 hours, so it can be inferred in theory that the continuous flow method can work continuously for 10 hours without changing the catalyst.
[0052] Table 2
[0053] Heterogeneous composite catalyst usage times 1 2 3 4 5 Vinyl sulfate yield% 81 80 80 79 79
[0054] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing vinyl sulfate using a continuous flow reaction system, characterized in that: The following steps are involved: Ethylene glycol and thionyl chloride are subjected to a cyclization reaction in a continuous flow reactor A, the product obtained by the cyclization reaction is subjected to a neutralization reaction with aqueous ammonia, and the product obtained after the neutralization reaction, an oxidant and a composite catalyst are subjected to an oxidation reaction in a continuous flow reactor B to obtain vinyl sulfate; the oxidant is sodium periodate; The composite catalyst comprises a carrier and ruthenium trichloride loaded on the carrier; the carrier is TiO2; the composite catalyst is obtained by reacting the carrier, a reducing agent and ruthenium trichloride in water; the reducing agent is selected from sodium borohydride.
2. The method according to claim 1, characterized in that: The continuous flow reaction system comprises a continuous flow reactor A and a continuous flow reactor B, and the continuous flow reactor A and the continuous flow reactor B both comprise a heat exchange layer and a reaction layer; The number of the continuous flow reaction systems connected in parallel is one or more.
3. The method according to claim 1, characterized in that: The mass ratio of ruthenium in ruthenium trichloride in the composite catalyst to the carrier is (0.0005-0.0015):
1.
4. The method according to claim 1, characterized in that The oxidation reaction specifically comprises mixing the product after the neutralization reaction with an oxidant and a composite catalyst in a continuous flow reaction system and performing an oxidation reaction at a temperature of 0-5°C.
5. The method according to claim 1, characterized in that In each continuous flow reaction system, the usage ratio of ethylene glycol, dichlorothionyl, ammonia water, oxidant and ruthenium in the composite catalyst every 2 to 4 hours is 4 mol: (4 to 4.2) mol: (8.03 to 8.99) mol: 4.02 mol: (0.00554 to 0.00633) mol.
6. The method according to claim 1, characterized in that The usage ratio of the carrier, the reducing agent, ruthenium trichloride and water is (500~1078) g: 10 g: 1280 mg: 30.2 L.
7. The method according to any one of claims 1 to 6, characterized in that: Ethylene glycol and thionyl chloride are mixed at a temperature of 0-5°C, and a cyclization reaction is carried out in a continuous flow reactor A at room temperature.