A high-strength and high-toughness PC / PBT alloy plastic and preparation method thereof

By using γ-glycidyl oxysilyl silsesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in PC/PBT alloy with hydroxylated glass fiber and nanographene oxide The combination of equal ingredients solves the problem of reduced mechanical properties and appearance defects caused by transesterification reaction, and achieves high-strength and high-toughness alloy properties and good spraying performance.

CN118290922BActive Publication Date: 2024-10-15SHANGHAI QISHEN ENG PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410719076.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-15
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

Existing PC/PBT alloys are prone to transesterification reactions during the high-temperature reactive melt blending process, resulting in reduced mechanical properties, and adding inorganic fillers can cause appearance defects such as silver threads or material flowers, affecting spraying performance.

Method used

The interface bonding component is used to form a macromolecular network structure from a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate and hydroxylated glass fiber. , combined with nanographene oxide and polybutadiene in the toughened emulsion, improves the compatibility and interface bonding strength of PC and PBT, and reduces transesterification reactions and degradation phenomena.

Benefits of technology

It improves the mechanical properties and toughness of PC/PBT alloy, reduces appearance defects, enhances spray plating performance, and meets high strength and high toughness requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of blended alloys, and specifically discloses a high-strength and high-toughness PC / PBT alloy plastic and a preparation method thereof. The PC / PBT alloy plastic comprises the following raw materials: polycarbonate, polybutylene terephthalate, a modifier, and an antioxidant; the modifier is prepared by mixing an interface bonding component and a toughening emulsion, and the interface bonding component is prepared by loading an interface improver and a phosphate heat-resistant agent on hydroxylated glass fiber; the toughening emulsion is prepared by emulsion polymerization of a toughening component having nano-graphene oxide as a core material, a silane monomer and an acrylate monomer, and polybutadiene as a wall material; and the preparation method comprises the following steps: drying polycarbonate and polybutylene terephthalate, mixing them with a modifier and an antioxidant, and then melt-blending them to obtain an alloy plastic. The present application has the characteristics of improving the mechanical properties of the PC / PBT alloy while solving the problem of silver wire or material flower defects in appearance due to the degradation of PC and PBT during processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of blended alloys, and more specifically, to a high-strength and high-toughness PC / PBT alloy plastic and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) is an amorphous polymer with a high glass transition temperature (about 145°C). As a high-performance hetero-chain thermoplastic engineering plastic, it is widely used in optics, medical equipment, films, etc. due to its excellent ductility and transparency. However, due to the high melt viscosity and poor processing fluidity of PC, it is usually prepared with some resins to improve the melt fluidity of PC.

[0003] Polybutylene terephthalate (PBT) is a semi-crystalline thermoplastic polymer with the highest crystallization rate, a low glass transition temperature, and a relatively high melting point (about 220°C). It is widely used in PC blending modification due to its excellent chemical corrosion resistance, mechanical properties, and better fluidity.

[0004] The modified PC / PBT alloy has good chemical resistance, mechanical properties and excellent processing fluidity. However, PC and PBT are prone to transesterification reaction under high temperature reactive melt blending. Although transesterification reaction can improve the compatibility between PC and PBT, the degree of reaction is usually uncontrollable in industrial production. As the degree of transesterification reaction increases, various complex copolymers such as block copolymers, random copolymers and random block copolymers will be formed, resulting in reduced mechanical properties of alloy plastics. In addition, in order to improve the strength of PC / PBT alloy to meet high strength requirements, inorganic fillers are added in related technologies. However, the addition of inorganic fillers will aggravate the transesterification reaction between PC and PBT, and the alkalinity of inorganic fillers will also cause PC and PBC resins to degrade during the blending process, making PC / PBT alloy prone to defects such as silver wire or material flowers, which leads to poor spraying and is difficult to meet product use requirements. Therefore, how to improve the mechanical properties of PC / PBT alloy while reducing the degradation of PC and PBT during processing to solve the problem of poor spraying is of great significance for the further promotion and application of PC / PBT alloy. Summary of the invention

[0005] In order to improve the mechanical properties of PC / PBT alloys while solving the problem of silver wire or material flower defects in appearance due to the degradation of PC and PBT during processing, the present application provides a high-strength and high-toughness PC / PBT alloy plastic and a preparation method thereof.

[0006] In the first aspect, the present application provides a high-strength and high-toughness PC / PBT alloy plastic, which adopts the following technical solution:

[0007] A high-strength and high-toughness PC / PBT alloy plastic, comprising the following raw materials in parts by weight:

[0008] 56-84 parts of polycarbonate, 24-36 parts of polybutylene terephthalate, 5-7 parts of modifier, 1-3 parts of antioxidant;

[0009] The modifier is prepared by mixing an interface bonding component and a toughening latex, the interface bonding component is prepared by loading an interface improver and a phosphate heat-resistant agent on hydroxylated glass fibers, and the interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate;

[0010] The toughening emulsion is prepared by emulsion polymerization with nano graphene oxide as core material, silane monomer and acrylate monomer and polybutadiene as wall material.

[0011] By adopting the above technical scheme, when polycarbonate and polybutylene terephthalate are melt-blended, since polycarbonate is in a non-crystalline state and polybutylene terephthalate is in a crystalline state, the interface bonding strength between the two is poor. During the melting process, an ester exchange reaction occurs between the two, which improves the compatibility of the two and causes the mechanical properties of the alloy to decrease. The addition of an antioxidant in the present application can improve the thermal stability of PC and PBT resins, reduce degradation during processing, and thus reduce the probability of defects such as silver wire or material flowers in the PC / PBT alloy. The addition of an interface bonding component in the modifier can improve the interface bonding performance of PC resin and PBT resin, inhibit the ester exchange reaction, and the addition of a toughening emulsion compensates for the reduction in mechanical properties of part of PC / PBT caused by the ester exchange reaction, thereby effectively reducing the reduction in the mechanical properties of the alloy. In addition, no alkaline filler is added to the raw material, so that while strengthening and toughening the PC / PBT alloy, it will not cause defects such as silver wire or material flowers in the PC / PBT alloy, which is more conducive to surface spraying and electroplating of the PC / PBT alloy.

[0012] In the present application, the interface bonding component is obtained by loading the hydroxylated glass fiber with the interface improver and the phosphate heat-resistant agent. When the interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate, the loaded fiber is firstly dispersed between the polycarbonate and the polybutylene terephthalate and penetrated therein through the dispersion effect, thereby connecting the polycarbonate and the polybutylene terephthalate. When melted at high temperature, the phosphate heat-resistant agent on the loaded fiber improves the heat resistance at the interface between the polycarbonate and the polybutylene terephthalate, further reducing the occurrence of ester exchange reaction, thereby reducing the adverse effects on the mechanical properties of the alloy.

[0013] More importantly, γ-glycidyl ether silyl propyl sesquioxane can enhance the compatibility between PC and PBT, allowing the two materials to be better integrated to form a stable alloy structure, improving the interfacial bonding strength between the two, and the introduction of silane groups in γ-glycidyl ether silyl propyl sesquioxane can improve the thermal stability of PC / PBT alloys, reduce their transesterification reaction under high temperature conditions and surface defects caused by high temperature degradation, improve the mechanical properties of PC / PBT alloys, and reduce the degradation of PC and PBT during processing to improve surface defects.

[0014] The introduction of biphenyl, ester bonds and ether groups into 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate and the introduction of benzene ring structure will increase the rigidity of the molecular chain, thereby improving the mechanical properties of the alloy such as tensile strength and bending modulus, thereby improving the mechanical properties of PC / PBT alloy. The ester bonds and ether groups form hydrogen bonding forces with the PC / PBT alloy, which not only improve the mechanical properties of the PC / PBT alloy but also play a stabilizing role. In addition, its epoxy group enables the load fiber to be smoothly dispersed and penetrated in polycarbonate and polybutylene terephthalate. The interface bonding part enables the loaded fiber to effectively improve the interface bonding strength of polycarbonate and polybutylene terephthalate, but the introduction of benzene ring groups will lead to a decrease in the toughness of the alloy, and γ-glycidyl ether silyl propyl sesquioxane helps to improve the toughness of the PC / PBT alloy by improving compatibility and thermal stability. In this application, the interface binder is a mixture of the two, which not only strengthens the PC / PBT alloy but also improves the toughness. Moreover, compared with inorganic filler reinforcement, it will not cause defects such as silver wire on the surface of the PC / PBT alloy due to alkalinity, affecting the spraying and electroplating performance.

[0015] Nano-graphene oxide and toughening components mainly composed of polybutadiene are added to the toughening emulsion. Nano-graphene oxide as a nanofiller can improve the compatibility with PC / PBT resin, reduce ester exchange and resin degradation, and does not contain alkalinity, which helps to improve the mechanical properties of the final product while reducing surface defects. The toughening component of polybutadiene further plays a toughening role. The final product has high strength and high toughness, which expands its application range and meets the requirements of high strength and high toughness.

[0016] Optionally, the phosphate heat-resistant agent is selected from one or both of (3-phenylallyl)-diethyl phosphate and 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate.

[0017] By adopting the above technical scheme, when the phosphate heat-resistant agent is selected from the above phosphate heat-resistant agent containing unsaturated functional groups, it can be polymerized with 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate when preparing the interface bonding component, and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate and γ-glycidyl ether silyl propyl sesquioxane can be chemically bonded with the hydroxylated glass fiber, so that the interface bonding component forms an overall macromolecular network structure, forming a whole, which is more helpful to improve the mechanical properties.

[0018] Optionally, the interface bonding component is prepared by the following steps:

[0019] The hydroxylated glass fiber is placed in anhydrous ethanol, and then an interface improver and a phosphate heat-resistant agent are added and mixed evenly, and then an initiator and a catalyst are added, condensed and refluxed, and after the initiator is dissolved, the temperature is raised to 80-90°C, the reaction is performed for 5-7 hours, cooled, centrifuged, and then vacuum dried to obtain an interface bonding component.

[0020] By adopting the above technical scheme, anhydrous ethanol is used as a medium to mix the interface improver and the phosphate heat-resistant agent with the hydroxylated glass fiber. Under the conditions of a catalyst and an initiator, the interface improver and the phosphate heat-resistant agent are chemically bonded to the hydroxylated glass fiber. Under the conditions of a catalyst, γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate are chemically bonded to the hydroxyl group through epoxy ring opening, so that the interface improver, the phosphate heat-resistant agent and the glass fiber are integrated, which is more conducive to entering the interface bonding of polycarbonate and polybutylene terephthalate during melt blending, and a macromolecular network structure is formed there, which further improves the interface bonding strength between the two and improves the mechanical properties of the product.

[0021] Optionally, during the preparation of the interface bonding component, the mass ratio of the hydroxylated glass fiber, the interface improver and the phosphate heat resistant agent added is 1: (0.6-0.8): (0.6-0.8);

[0022] The added mass ratio of γ-glycidyl ether silyl propyl sesquioxane to 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in the interface improver is 1:(0.8-1);

[0023] The initiator is added in an amount of 1-3wt% of the hydroxylated glass fiber;

[0024] The catalyst addition amount is 0.3-0.5wt% of the hydroxylated glass fiber.

[0025] By adopting the above technical solution and selecting the raw materials with the above ratio, the comprehensive performance of strength and toughness of the final product is better.

[0026] Optionally, the toughening emulsion is prepared by the following method:

[0027] Ultrasonic dispersion of nano-graphene oxide, surfactant, PVA and the first portion of water for 20-30 minutes to prepare a nano-graphene oxide suspension;

[0028] Mix the acrylate monomer and the silane monomer, heat to 65-75°C, then add a mixed solution of a catalyst, an emulsifier and a second portion of water, then add a nano-graphene oxide suspension and an initiator, react under high-speed shear conditions for 2-3 hours, then add polybutadiene, continue to react for 1-2 hours, cool and stand, and wash to obtain a toughened emulsion.

[0029] By adopting the above technical scheme, in the present application, butyl acrylate, methacryloyloxypropyl trimethoxysilane, vinyl phenyl dimethoxy silane and methacrylate glycidyl ester are used as monomers, and after adding nano graphene oxide suspension, in an emulsified system, under the action of an initiator, the above monomers form a polymer wall material on the surface of nano graphene oxide through a polymerization reaction, and then polybutadiene is added. Under the action of an initiator and a catalyst, the polybutadiene is grafted and copolymerized with a polyacrylate-polysiloxane copolymer to achieve the modification of nano graphene oxide, and on the surface The toughening component polybutadiene is introduced to provide toughening effect in the modifier, and nano-graphene oxide is used to achieve the toughening and strengthening effect on PC / PBT. In addition, acrylate and siloxane monomers are added to the monomer at the same time. The addition of siloxane monomer helps to improve its compatibility with the interface bonding component, while the addition of acrylate monomer helps to improve the compatibility of polysiloxane and polybutadiene, forming a stable microcapsule structure, and also improves the compatibility of polybutadiene with polycarbonate and polybutylene terephthalate, thereby improving the mechanical properties of the alloy plastic.

[0030] When preparing nano-graphene oxide suspension, the addition of surfactant reduces the surface tension of the mixed solution, making nano-graphene oxide easier to disperse, and the addition of PVA inhibits the agglomeration of nano-graphene oxide in the solution, thereby making the suspension more stable.

[0031] Optionally, the acrylate monomer is selected from any one or more of butyl acrylate, glycidyl methacrylate and triethylene glycol dimethacrylate;

[0032] The silane monomer is selected from any one or more of methacryloxypropyltrimethoxysilane, vinylphenyldimethoxysilane and acryldiphenylmethoxysilane.

[0033] Optionally, the acrylic acid ester monomer is a mixture of butyl acrylate and glycidyl methacrylate in a mass ratio of 1:(0.6-0.8);

[0034] Optionally, the silane monomer is a mixture of methacryloxypropyltrimethoxysilane and vinylphenyldimethoxysilane in a mass ratio of 1:(2-3).

[0035] Optionally, in the step of preparing the toughening emulsion, the amount of each raw material added is as follows:

[0036] 40-50 parts of nano-graphene oxide, 5-8 parts of surfactant, 1-3 parts of PVA, 30-40 parts of the first part of water, 20-30 parts of acrylate monomer, 15-25 parts of silane monomer, 1-3 parts of catalyst, 8-15 parts of emulsifier, 10-15 parts of the second part of water, 3-5 parts of initiator, and 10-20 parts of polybutadiene.

[0037] Optionally, the modifier is prepared by the following steps:

[0038] The interface bonding component and the toughening emulsion are mixed, heated in a water bath at 55-65° C. for 1-2 hours to obtain a mixed solution, and then a magnesium sulfate solution is added to break the emulsion. After the emulsion is broken, the solution is filtered and dried to obtain a modifier.

[0039] By adopting the above technical scheme, in the present application, the interface bonding component is mixed with the toughening solution and then demulsified in a magnesium sulfate solution. The graphene oxide forms a good and stable interaction with the polymer wall material through functional groups such as surface hydroxyl groups, so that the nano graphene oxide is still wrapped inside by the polymer after demulsification, and the structure of the polymer wrapped graphene is maintained. The structure is loaded on the interface bonding component after demulsification to form a larger agglomerate, so that the polymer particles are precipitated, and then separated to obtain the modifier. During the melting process of the prepared PC / PBT alloy, the toughening component arrives at the interface bonding position of polycarbonate and polybutylene terephthalate along with the interface bonding component, thereby improving the mechanical properties of polycarbonate and polybutylene terephthalate.

[0040] Optionally, the interface bonding component and the toughening emulsion are added in a weight ratio of 2:(3-5), and the amount of magnesium sulfate solution added is 20-30 wt% of the mixed solution.

[0041] In a second aspect, the present application provides a method for preparing a high-strength and high-toughness PC / PBT alloy plastic, using the following technical solution:

[0042] A method for preparing high-strength and high-toughness PC / PBT alloy plastic comprises the following steps: drying polycarbonate and polybutylene terephthalate, mixing them with a modifier and an antioxidant, and then melting and blending them to obtain the alloy plastic.

[0043] By adopting the above technical solution, the modifier is added to polycarbonate and polybutylene terephthalate. During the melting process, the toughening component arrives at the interface of polycarbonate and polybutylene terephthalate along with the interface bonding component, thereby improving the mechanical properties of polycarbonate and polybutylene terephthalate.

[0044] In summary, this application has the following beneficial effects:

[0045] 1. The addition of the interface bonding component in the modifier of the present application can improve the interface bonding performance of PC resin and PBT resin, inhibit the ester exchange reaction, and the addition of the toughening emulsion can compensate for the reduction in mechanical properties of PC / PBT caused by the ester exchange reaction, thereby effectively reducing the reduction in mechanical properties of the alloy. In addition, no alkaline filler is added to the raw material, which can achieve the enhancement and toughening of the PC / PBT alloy without causing defects such as silver wire or material flower in the PC / PBT alloy, which is more conducive to the surface spraying and electroplating of the PC / PBT alloy;

[0046] 2. In the present application, the interface bonding component is obtained by loading the hydroxylated glass fiber with the interface modifier and the phosphate heat-resistant agent. When the interface modifier is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate, the loaded fiber is firstly dispersed between the polycarbonate and the polybutylene terephthalate through the dispersion effect and penetrates therein, thereby connecting the polycarbonate and the polybutylene terephthalate. When melted at high temperature, the phosphate heat-resistant agent on the loaded fiber improves the heat resistance at the interface of the polycarbonate and the polybutylene terephthalate, further reducing the occurrence of the ester exchange reaction, thereby reducing the adverse effects on the mechanical properties of the alloy;

[0047] 3. In the present application, γ-glycidyl ether silyl propyl sesquioxane can enhance the compatibility between PC and PBT, so that the two materials can be better integrated to form a stable alloy structure, and the interfacial bonding strength between the two can be improved. Moreover, the introduction of silane groups in γ-glycidyl ether silyl propyl sesquioxane can improve the thermal stability of PC / PBT alloy, reduce its transesterification reaction under high temperature conditions and the occurrence of surface defects due to high temperature degradation, improve the mechanical properties of PC / PBT alloy, and reduce the degradation of PC and PBT during processing to improve the problem of surface defects;

[0048] 4. In the present application, biphenyl, ester bonds and ether groups are introduced into 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate. The introduction of the benzene ring structure will increase the rigidity of the molecular chain, thereby improving the mechanical properties of the alloy such as tensile strength and bending modulus, thereby improving the mechanical properties of the PC / PBT alloy. The ester bonds and ether groups form hydrogen bonding forces with the PC / PBT alloy, which not only improves the mechanical properties of the PC / PBT alloy but also plays a stabilizing role. In addition, the epoxy group enables the load fiber to be smoothly dispersed and penetrated in the polycarbonate and polyethylene terephthalate. The interface bonding of polybutylene terephthalate enables the loaded fiber to effectively improve the interface bonding strength of polycarbonate and polybutylene terephthalate, but the introduction of benzene ring groups will lead to a decrease in the toughness of the alloy, and γ-glycidyl ether silyl propyl sesquioxane helps to improve the toughness of the PC / PBT alloy by improving compatibility and thermal stability. In this application, the interface binder is a mixture of the two, which not only enhances the toughness, but also enhances the toughness. Compared with the inorganic filler enhancement, it will not cause defects such as silver wire on the surface of the PC / PBT alloy due to alkalinity, affecting the spraying and electroplating performance;

[0049] 5. The toughening emulsion of the present application contains nano-graphene oxide and toughening components mainly composed of polybutadiene. Nano-graphene oxide as a nanofiller can improve the compatibility with PC / PBT resin, reduce ester exchange and resin degradation, and does not contain alkalinity, thereby helping to improve the mechanical properties of the final product while reducing surface defects. The toughening component of polybutadiene further plays a toughening role. The final product has high strength and high toughness, which expands its application range and meets the requirements of high strength and high toughness. DETAILED DESCRIPTION

[0050] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0051] The percentages in the following examples are by mass unless otherwise specified.

[0052] In the following preparation examples, nano-graphene oxide is selected from Suzhou Kaifa New Material Technology Co., Ltd., with model number szbknm2010 and product number NGO1511.

[0053] In the following examples, the antioxidant selected is antioxidant 1010;

[0054] In the following examples, the polycarbonate PC is Luxi Chemical PC 1920T with a flexural modulus of 3500 MPa; the polybutylene terephthalate PBT is Kanghui Petrochemical PBT KH2083 with a melt index of 43 g / 10 min.

[0055] In the present application, 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate is prepared by the following steps:

[0056] Under argon protection, add 2.98g 4,4'-biphenyl diglycidyl ether, 5.17g methacrylic acid, and 0.03g N,N-dimethylbenzylamine to a 100mL four-necked reaction bottle, raise the reaction temperature to 95°C, react for 12h, and stop the reaction. The reaction solution is cooled to room temperature, 50mL dichloroethane is added to dissolve, and then washed alternately with NaOH and 60°C water three times, then dried over anhydrous MgSO4, filtered, and the solvent is removed by spinning to obtain a light yellow solid.

[0057] The following preparation example is a preparation example of a modifier:

[0058] Preparation Example 1

[0059] S1. Preparation of interface bonding components: The specific operations are as follows:

[0060] S1-1, placing 200g of glass fiber in a muffle furnace, keeping the temperature at 500℃ for 3h, then adding 1L of 65% nitric acid, reacting at 70℃ for 5h, washing it with 50% ethanol aqueous solution to neutrality, and then placing it in a vacuum drying oven at 80℃ for 12h to obtain hydroxylated glass fiber;

[0061] S1-2, weigh 1 kg of the hydroxylated glass fiber obtained in step S1-1 and place it in 30 L of anhydrous ethanol, then add the interface improver and the phosphate heat-resistant agent, stir for 10 min to mix evenly, then add the initiator and the catalyst, condense and reflux, stir at 50 ° C for 20 min, raise the temperature to 85 ° C after the initiator is dissolved, react for 6 h, cool, centrifuge, and then vacuum dry to obtain the interface bonding component;

[0062] Among them, the added mass ratio of hydroxylated glass fiber, interface improver and phosphate heat resistant agent is 1:0.7:0.7;

[0063] The interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in a mass ratio of 1:0.9;

[0064] The phosphate heat-resistant agent is (3-phenylallyl)-diethyl phosphate;

[0065] The initiator is dibenzoyl peroxide, and the amount of the initiator added is 2wt% of the hydroxylated glass fiber. The catalyst is triethylamine and zinc octanoate in a mass ratio of 1:1, and the amount of the catalyst added is 0.4wt% of the hydroxylated glass fiber.

[0066] S2. Preparation of toughening component: specifically including the following operations:

[0067] S2-1, 45 kg of nano-graphene oxide, 6 kg of surfactant sodium dodecyl sulfate, 2 kg of PVA and 35 kg of the first part of water were ultrasonically dispersed for 25 min at an ultrasonic power of 40 W to obtain a nano-graphene oxide suspension;

[0068] S2-2, 25 kg of acrylate monomer and 20 kg of silane monomer were mixed, the temperature was raised to 70° C., and then a mixed solution of 2 kg of catalyst, 12 kg of emulsifier and 12 kg of the second part of water was added, and then the nano-graphene oxide suspension prepared in step S2-1 and 4 kg of initiator were added, and 15 kg of polybutadiene was added after reacting for 2.5 hours under high-speed shear conditions of 13000 rpm, and the reaction was continued for 1.5 hours, cooled and allowed to stand, and a toughened emulsion was obtained after washing;

[0069] The acrylate monomer is a mixture of butyl acrylate and glycidyl methacrylate in a mass ratio of 1:0.7, and the silane monomer is a mixture of methacryloyloxypropyl trimethoxysilane and vinylphenyl dimethoxysilane in a mass ratio of 1:2.5.

[0070] The catalyst is cumene hydroperoxide, the emulsifier is polyoxypropylene ether, and the initiator is azobisisobutyronitrile;

[0071] S3, preparing a modifier: taking the interface bonding component prepared in step S1 and the toughening emulsion prepared in step S2 in a mass ratio of 2:4, mixing them, heating them in a water bath at 60°C for 1.5h to obtain a mixed solution, and then adding a magnesium sulfate solution with a mass fraction of 5wt% to break the emulsion, the magnesium sulfate solution is added in an amount of 25wt% of the mixed solution, and filtering and drying after breaking the emulsion to obtain a modifier.

[0072] Preparation Example 2

[0073] S1. Preparation of interface bonding components: The specific operations are as follows:

[0074] S1-1, placing 150g of glass fiber in a muffle furnace, keeping the temperature at 480℃ for 3.5h, then adding 1L of 65% nitric acid, reacting at 65℃ for 5.5h, washing it with 50% ethanol aqueous solution to neutrality, and then placing it in a vacuum drying oven at 75℃ for 13h to obtain hydroxylated glass fiber;

[0075] S1-2, weigh 1 kg of the hydroxylated glass fiber obtained in step S1-1 and place it in 30 L of anhydrous ethanol, then add the interface improver and the phosphate heat-resistant agent, stir for 10 min to mix evenly, then add the initiator and the catalyst, condense and reflux, stir at 45 ° C for 30 min, raise the temperature to 80 ° C after the initiator is dissolved, react for 7 h, cool, centrifuge, and then vacuum dry to obtain the interface bonding component;

[0076] Among them, the added mass ratio of hydroxylated glass fiber, interface improver and phosphate heat resistant agent is 1:0.6:0.6;

[0077] The interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in a mass ratio of 1:0.8;

[0078] The phosphate heat-resistant agent is 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate;

[0079] The initiator is dibenzoyl peroxide, and the amount of the initiator added is 1wt% of the hydroxylated glass fiber. The catalyst is triethylamine and zinc octanoate in a mass ratio of 1:1, and the amount of the catalyst added is 0.3wt% of the hydroxylated glass fiber.

[0080] S2. Preparation of toughening component: specifically including the following operations:

[0081] S2-1, 40 kg of nano-graphene oxide, 5 kg of surfactant sodium dodecyl sulfate, 1 kg of PVA and 30 kg of the first part of water were ultrasonically dispersed for 20 min at an ultrasonic power of 40 W to obtain a nano-graphene oxide suspension;

[0082] S2-2, 20 kg of acrylate monomer and 15 kg of silane monomer were mixed, the temperature was raised to 65° C., and then a mixed solution of 1 kg of catalyst, 8 kg of emulsifier and 10 kg of the second part of water was added, and then the nano-graphene oxide suspension prepared in step S2-1 and 3 kg of initiator were added, and 10 kg of polybutadiene was added after reacting for 3 hours under high-speed shear conditions of 12000 rpm, and the reaction was continued for 1 hour, cooled and allowed to stand, and a toughened emulsion was obtained after washing;

[0083] The acrylate monomer is a mixture of butyl acrylate and glycidyl methacrylate in a mass ratio of 1:0.6, and the silane monomer is a mixture of methacryloyloxypropyl trimethoxysilane and vinylphenyl dimethoxysilane in a mass ratio of 1:2.

[0084] The catalyst is cumene hydroperoxide, the emulsifier is polyoxyethylene ether, and the initiator is azobisisobutyronitrile;

[0085] S3. Preparation of a modifier: The interfacial bonding component prepared in step S1 and the toughening emulsion prepared in step S2 are mixed in a mass ratio of 2:3, heated in a water bath at 55° C. for 2 h to obtain a mixed solution, and then a 5wt% magnesium sulfate solution is added for demulsification, wherein the amount of magnesium sulfate solution added is 20wt% of the mixed solution. After demulsification, the mixture is filtered and dried to obtain a modifier.

[0086] Preparation Example 3

[0087] S1. Preparation of interface bonding components: The specific operations are as follows:

[0088] S1-1, placing 250g of glass fiber in a muffle furnace, keeping the temperature at 550℃ for 2.5h, then adding 1L of 65% nitric acid by mass, reacting at 75℃ for 4h, washing it with 50% ethanol aqueous solution by volume until it is neutral, and then placing it in a vacuum drying oven at 85℃ for 11h to obtain hydroxylated glass fiber;

[0089] S1-2, weigh 1 kg of the hydroxylated glass fiber obtained in step S1-1 and place it in 30 L of anhydrous ethanol, then add the interface improver and the phosphate heat-resistant agent, stir for 10 min to mix evenly, then add the initiator and the catalyst, condense and reflux, stir at 55 ° C for 25 min, raise the temperature to 90 ° C after the initiator is dissolved, react for 5 h, cool, centrifuge, and then vacuum dry to obtain the interface bonding component;

[0090] Among them, the added mass ratio of hydroxylated glass fiber, interface improver and phosphate heat resistant agent is 1:0.8:0.8;

[0091] The interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in a mass ratio of 1:1.

[0092] The phosphate heat-resistant agent is (3-phenylallyl)-diethyl phosphate;

[0093] The initiator is dibenzoyl peroxide, and the amount of the initiator added is 3wt% of the hydroxylated glass fiber. The catalyst is triethylamine and zinc octanoate in a mass ratio of 1:1, and the amount of the catalyst added is 0.5wt% of the hydroxylated glass fiber.

[0094] S2. Preparation of toughening component: specifically including the following operations:

[0095] S2-1, 50 kg of nano-graphene oxide, 8 kg of surfactant sodium dodecyl sulfate, 3 kg of PVA and 40 kg of the first part of water were ultrasonically dispersed for 30 min at an ultrasonic power of 40 W to obtain a nano-graphene oxide suspension;

[0096] S2-2, 30 kg of acrylate monomer and 25 kg of silane monomer were mixed, the temperature was raised to 75° C., and then a mixed solution of 3 kg of catalyst, 15 kg of emulsifier and 15 kg of the second part of water was added, and then the nano-graphene oxide suspension prepared in step S2-1 and 5 kg of initiator were added, and 20 kg of polybutadiene was added after reacting for 2 hours under high-speed shear conditions of 14000 rpm, and the reaction was continued for 2 hours, cooled and allowed to stand, and a toughened emulsion was obtained after washing;

[0097] The acrylate monomer is a mixture of butyl acrylate and glycidyl methacrylate in a mass ratio of 1:0.8, and the silane monomer is a mixture of methacryloyloxypropyl trimethoxysilane and vinylphenyl dimethoxysilane in a mass ratio of 1:3.

[0098] The catalyst is cumene hydroperoxide, the emulsifier is polyoxypropylene ether, and the initiator is azobisisobutyronitrile;

[0099] S3, preparing a modifier: taking the interface bonding component prepared in step S1 and the toughening emulsion prepared in step S2 in a mass ratio of 2: 5, mixing them, heating them in a water bath at 65°C for 1h to obtain a mixed solution, then adding a magnesium sulfate solution with a mass fraction of 5wt% to break the emulsion, the magnesium sulfate solution is added in an amount of 30wt% of the mixed solution, filtering and drying after breaking the emulsion, and obtaining a modifier.

[0100] Preparation Example 4

[0101] The modifier was prepared according to the method in Preparation Example 1, except that in step S3, the interface bonding component prepared in step S1 and the toughening emulsion prepared in step S2 were mixed in a mass ratio of 2:5, and then directly dried without performing a demulsification operation to obtain the modifier.

[0102] Preparation Example 5

[0103] The modifier was prepared according to the method in Preparation Example 1, except that isodecyl alcohol polyoxyethylene ether phosphate was used as the phosphate heat-resistant agent.

[0104] Preparation Example 6

[0105] The modifier was prepared according to the method in Preparation Example 1, except that the interface bonding component was prepared by directly mixing the hydroxylated glass fiber, the interface improving agent and the phosphate heat resistant agent, and then vacuum drying.

[0106] Comparative Preparation Example 1

[0107] The modifier was prepared according to the method in Preparation Example 1, except that the hydroxylated glass fibers in the interface bonding component were directly replaced by glass fibers in equal amounts.

[0108] Comparative Preparation Example 2

[0109] The modifier was prepared according to the method in Preparation Example 1, except that γ-glycidyl ether silyl propyl sesquioxane was used as the interface improver.

[0110] Comparative Preparation Example 3

[0111] The modifier was prepared according to the method in Preparation Example 1, except that 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate was used as the interface improver.

[0112] Comparative Preparation Example 4

[0113] The modifier was prepared according to the method in Preparation Example 1, except that the interface improver in the interface bonding component was replaced by an equal amount of a phosphate heat-resistant agent.

[0114] Comparative Preparation Example 5

[0115] The modifier was prepared according to the method of Preparation Example 1, except that an equal amount of γ-glycidyloxysilylpropylsesquioxane was replaced by sodium dodecyl sulfate.

[0116] Comparative Preparation Example 6

[0117] The modifier was prepared according to the method in Preparation Example 1, except that in the step of preparing the toughening emulsion, the silane monomer was replaced by an acrylate monomer in equal amounts.

[0118] Comparative Preparation Example 7

[0119] The modifier was prepared according to the method in Preparation Example 1, except that the toughening latex was prepared by the following method:

[0120] S1. Under nitrogen protection, the water bath heating temperature is 70°C, the stirring speed is 280r / min, 1500g deionized water and 2.5g sodium pyrophosphate are mixed, and the sodium pyrophosphate is dissolved;

[0121] S2, adding 3.5 g of glucose, 0.05 g of ferrous sulfate, 550 g of polybutadiene latex, 0.5 g of potassium hydroxide and 1.5 g of cumene hydroperoxide to the mixed solution in S1 in sequence;

[0122] S3, continue to drop 265g styrene, 90g methyl methacrylate and 10g glycidyl methacrylate; finish the reaction 2 hours after the dropwise addition to obtain a toughened emulsion.

[0123] Comparative Preparation Example 8

[0124] A modifier was prepared according to the method in Preparation Example 1, except that 45 kg of nano-graphene oxide was directly mixed with 15 kg of polybutadiene and allowed to stand, then filtered and dried to obtain a toughening component, and then the toughening component was directly mixed with the interface bonding component obtained in step S1 at a mass ratio of 4:2 to obtain a modifier.

[0125] Comparative Preparation Example 9

[0126] The modifier was prepared according to the method in Preparation Example 1, except that an equal amount of nano-graphene oxide was replaced by nano-graphene.

[0127] Example 1

[0128] A method for preparing high-strength and high-toughness PC / PBT alloy plastic comprises the following steps:

[0129] S1, placing polycarbonate and polybutylene terephthalate in an electric blast drying oven at a constant temperature of 120° C. and drying for 4 h to remove moisture, and using a high-speed mixer to uniformly mix 65 kg of polycarbonate, 30 kg of polybutylene terephthalate, 2 kg of antioxidant 1010 and 6 kg of the modifier prepared in Preparation Example 1;

[0130] S2. Pour the mixture into a twin-screw extruder, melt-blend the melt in each zone, extrude it from the die, cool it with water and pull it with a traction machine for pelletizing, thus achieving melt-blending and extrusion pelletizing to obtain PC / PBT alloy plastic.

[0131] Example 2

[0132] A method for preparing high-strength and high-toughness PC / PBT alloy plastic comprises the following steps:

[0133] S1, placing polycarbonate and polybutylene terephthalate in an electric blast drying oven at a constant temperature of 120° C. for 4 h to remove moisture, and using a high-speed mixer to uniformly mix 56 kg of polycarbonate, 24 kg of polybutylene terephthalate, 1 kg of antioxidant 1010 and 5 kg of the modifier prepared in Preparation Example 2;

[0134] S2. Pour the mixture into a twin-screw extruder, melt-blend the melt in each zone, extrude it from the die, cool it with water and pull it with a traction machine for pelletizing, thus achieving melt-blending and extrusion pelletizing to obtain PC / PBT alloy plastic.

[0135] Example 3

[0136] A method for preparing high-strength and high-toughness PC / PBT alloy plastic comprises the following steps:

[0137] S1, placing polycarbonate and polybutylene terephthalate in an electric blast drying oven at a constant temperature of 120° C. and drying for 4 h to remove moisture, and using a high-speed mixer to uniformly mix 84 kg of polycarbonate, 36 kg of polybutylene terephthalate, 3 kg of antioxidant 1010 and 7 kg of the modifier prepared in Preparation Example 3;

[0138] S2. Pour the mixture into a twin-screw extruder, melt-blend the melt in each zone, extrude it from the die, cool it with water and pull it with a traction machine for pelletizing, thus achieving melt-blending and extrusion pelletizing to obtain PC / PBT alloy plastic.

[0139] Embodiment 4-6

[0140] A method for preparing high-strength and high-toughness PC / PBT alloy plastic, the difference being that the modifiers are respectively selected from the modifiers prepared in Preparation Examples 4-6.

[0141] Comparative Example 1

[0142] A method for preparing high-strength and high-toughness PC / PBT alloy plastic, the difference being that no modifier is added to the raw materials.

[0143] Comparative Examples 2-10

[0144] A method for preparing high-strength and high-toughness PC / PBT alloy plastic, the difference being that the modifiers in the raw materials are respectively selected from the modifiers prepared in comparative preparation examples 1-9.

[0145] Performance Testing

[0146] The PC / PBT alloy plastics prepared in the above examples and comparative examples were observed for appearance defects such as silver threads or material flowers. In addition, tensile properties, bending properties and notched impact properties were tested, as follows:

[0147] Tensile property test: According to ISO 527-1-2012, the tensile test was carried out using an electronic universal testing machine. A dumbbell-shaped specimen was selected, with a length of 150 mm, a width of 10 mm, and a thickness of 4 mm, and the test rate was 50 mm / min.

[0148] Bending performance test: According to ISO 178-2010, the bending strength is determined by a three-point bending test using an electronic universal testing machine. A sample with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm is selected, and the test rate is 2 mm / min.

[0149] Notch impact performance test: refer to GB 1043-70 for testing, the alloy plastic is injection molded into dumbbell-shaped specimens with a length of 55mm, a width of 10mm and a thickness of 4mm. A notched specimen is made on a ZHY-W universal prototype making machine, and the notch depth is one-third of the specimen thickness.

[0150] The test results are shown in Table 1 below.

[0151] Table 1:

[0152]

[0153] According to the test results in Table 1 above, the PC / PBT alloy plastic obtained in the embodiment of the present application has excellent tensile strength, flexural strength and notched impact strength, has excellent mechanical properties, and has better toughness while being enhanced. Combining the test results of Example 1 and Example 4, it can be seen that when the interface bonding component and the toughening emulsion are directly dried without demulsification, the mechanical properties of the PC / PBT alloy plastic are reduced. It can be seen that the toughening emulsion is combined with the interface bonding component, and the toughening component is loaded on the interface bonding component after demulsification. During the melting process, the toughening component arrives at the interface bonding of polycarbonate and polybutylene terephthalate with the interface bonding component, thereby improving the mechanical properties of polycarbonate and polybutylene terephthalate.

[0154] Referring to the test results of Example 1 and Example 5, when the phosphate heat-resistant agent in the interface bonding component is a saturated phosphate, the mechanical properties of the PC / PBT alloy plastic obtained in the end are reduced. The phosphate heat-resistant agent containing an unsaturated bond can form a chemical bond with the hydroxylated glass fiber, and can also continue to polymerize with 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate and γ-glycidyl ether oxygen silyl propyl sesquioxane, so that the interface bonding component forms an overall macromolecular network structure, thereby enhancing the mechanical properties of the PC / PBT alloy plastic.

[0155] Combined with the test results of Example 1 and Example 6, when the hydroxylated glass fiber, the interface improvement and the phosphate heat resistant agent are directly mixed without initiating the reaction with an initiator, the mechanical properties of the PC / PBT alloy plastic finally obtained are significantly reduced compared to the physical mixing in Example 1. Adding an initiator and a catalyst and reacting at a high temperature helps to form a macromolecular network structure, thereby improving the mechanical properties of the PC / PBT alloy plastic.

[0156] Combining the test results of Example 1 and Comparative Example 1, it can be seen that when no modifier is added to the raw material, when the PC / PBT alloy plastic is obtained, its mechanical properties are low, and silver wire and material flower defects appear in the appearance, which is not conducive to the subsequent spraying and electroplating operations. Combined with the test results of Comparative Example 2, when the hydroxylated glass fiber is directly replaced with glass fiber in equal amounts, the mechanical properties of the obtained alloy plastic are reduced. Referring to the test results of Comparative Examples 3 and 4, it can be seen that the interface improver only uses γ-glycidyl ether oxysilyl propyl sesquioxane or 4,4'-biphenyl bisphenol diglycidyl ether When dimethacrylate is used, its mechanical properties are relatively low, especially when only γ-glycidyl ether silyl propyl sesquioxane is added in Comparative Example 3, the mechanical properties are significantly reduced; referring to the test results of Comparative Example 5, when only phosphate heat-resistant agent is added to the interface bonding component without adding an interface modifier, its mechanical properties are significantly reduced, and a small amount of silver wire and material flower defects appear in the appearance; and when an equal amount of γ-glycidyl ether silyl propyl sesquioxane is replaced with a common dispersant of sodium dodecyl sulfate in Comparative Example 6, the mechanical properties are significantly reduced, and a small amount of silver wire and material flower defects also appear in the appearance;

[0157] Referring to Comparative Example 7, when no silane monomer is added to the toughening emulsion and only acrylate monomer is added, when the mechanical properties are reduced, there are a small amount of silver wire and material flower defects in the appearance. In Comparative Example 8, when no nano-graphene oxide is added to the toughening emulsion, but only polystyrene and acrylate and other toughening components are added, it can be seen that the tensile strength of the alloy plastic finally obtained is significantly reduced, the toughness is also slightly reduced, and a small amount of silver wire and material flower defects appear in the appearance. In Comparative Example 9, when the toughening component is selected from nano-graphene oxide and directly loaded with polybutadiene components, the strength and toughness are reduced, and the appearance of silver wire and material flower defects is more obvious. In Comparative Example 10, when nano-graphene oxide is replaced by nano-graphene in equal amounts, the mechanical properties are significantly reduced, mainly because when graphene is emulsion-polymerized with silane monomers and acrylic monomers and then demulsified, the oil phase wall material is separated from the inorganic core material graphene, resulting in poor graphene dispersion, a significant reduction in mechanical properties, and silver wire and material flower defects in appearance.

[0158] In summary, in this application, in order to address the current ester exchange that leads to reduced mechanical properties and the appearance of silver threads and material flowers, on the one hand, an interface bonding component of specific composition is used, so that γ-glycidyl ether silylpropyl sesquioxane, 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate and hydroxylated fibers form a macromolecular network structure and form a whole, so that the overall stability of the interface bonding component is improved, and the interface bonding effect of PC and PBT is better exerted. In addition, nano-graphene oxide is used in the toughening emulsion to play a reinforcing role, and acrylic monomers and silane monomers are used through emulsion polymerization and graft polymerization of polybutadiene and other toughening components, which can significantly improve the appearance defects while achieving reinforcement and toughening.

[0159] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high-strength and high-toughness PC / PBT alloy plastic, It is characterized in that The invention comprises the following raw materials in parts by weight: 56-84 parts of polycarbonate, 24-36 parts of polybutylene terephthalate, 5-7 parts of modifier, 1-3 parts of antioxidant; The modifier is prepared by mixing an interface bonding component and a toughening latex, the interface bonding component is prepared by loading an interface improver and a phosphate heat-resistant agent on hydroxylated glass fibers, and the interface improver is a mixture of γ-glycidyl ether silyl propyl sesquioxane and 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate; The toughening emulsion is prepared by emulsion polymerization with nano graphene oxide as core material, silane monomer and acrylate monomer and polybutadiene as wall material toughening components; The interface bonding component is prepared by the following steps: The hydroxylated glass fiber is placed in anhydrous ethanol, and then an interface improver and a phosphate heat-resistant agent are added and mixed evenly, and then an initiator and a catalyst are added, condensed and refluxed, and after the initiator is dissolved, the temperature is raised to 80-90° C., reacted for 5-7 hours, cooled, centrifuged, and then vacuum dried to obtain an interface bonding component; The toughening emulsion is prepared by the following method: Ultrasonic dispersion of nano-graphene oxide, surfactant, PVA and the first portion of water for 20-30 minutes to prepare a nano-graphene oxide suspension; Mix the acrylate monomer and the silane monomer, raise the temperature to 65-75° C., then add the catalyst, the emulsifier and the mixed solution of the second part of water, then add the nano-graphene oxide suspension and the initiator, react under high-speed shear conditions for 2-3 hours, then add polybutadiene, continue to react for 1-2 hours, cool and stand, and wash to obtain a toughened emulsion; The modifying agent is prepared by the following steps: The interface bonding component and the toughening emulsion are mixed, heated in a water bath at 55-65° C. for 1-2 hours to obtain a mixed solution, and then a magnesium sulfate solution is added to break the emulsion. After the emulsion is broken, the solution is filtered and dried to obtain a modifier.

2. A high-strength and high-toughness PC / PBT alloy plastic according to claim 1, Features: The phosphate heat-resistant agent is selected from one or both of (3-phenylallyl)-diethyl phosphate and 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate.

3. The high-strength and high-toughness PC / PBT alloy plastic according to claim 1, Features: During the preparation of the interface bonding component, the added mass ratio of hydroxylated glass fiber, interface improver and phosphate heat resistant agent is 1: (0.6-0.8): (0.6-0.8); The added mass ratio of γ-glycidyl ether silyl propyl sesquioxane to 4,4'-biphenyl bisphenol diglycidyl ether dimethacrylate in the interface improver is 1:(0.8-1); The initiator is added in an amount of 1-3wt% of the hydroxylated glass fiber; The catalyst addition amount is 0.3-0.5wt% of the hydroxylated glass fiber.

4. The high-strength and high-toughness PC / PBT alloy plastic according to claim 1, Features: The acrylate monomer is selected from any one or more of butyl acrylate, glycidyl methacrylate and triethylene glycol dimethacrylate; The silane monomer is selected from any one or more of methacryloxypropyltrimethoxysilane, vinylphenyldimethoxysilane and acryldiphenylmethoxysilane.

5. The high-strength and high-toughness PC / PBT alloy plastic according to claim 1, Features: In the toughening emulsion preparation step, the amount of each raw material added is as follows: 40-50 parts of nano-graphene oxide, 5-8 parts of surfactant, 1-3 parts of PVA, 30-40 parts of the first part of water, 20-30 parts of acrylate monomer, 15-25 parts of silane monomer, 1-3 parts of catalyst, 8-15 parts of emulsifier, 10-15 parts of the second part of water, 3-5 parts of initiator, and 10-20 parts of polybutadiene.

6. The high-strength and high-toughness PC / PBT alloy plastic according to claim 1, Features: The weight ratio of the interface bonding component to the toughening emulsion is 2:(3-5), and the amount of magnesium sulfate solution added is 20-30 wt% of the mixed solution.

7. A method for preparing a high-strength and high-toughness PC / PBT alloy plastic according to any one of claims 1 to 6, Features: The following steps are involved: The polycarbonate and polybutylene terephthalate are dried, mixed with a modifier and an antioxidant, and then melt-blended to obtain an alloy plastic.