A polyurethane material for charging pile cable

Through the combination of modified polyurethane matrix material and elastic particle fiber, the problem of outer sheath rupture caused by bending of charging pile cables is solved, the bending resistance and mechanical properties of the cable are improved, and the cable life is extended.

CN118290931BActive Publication Date: 2024-10-01SHANGHAI JIELI NEW MATERIALS TECHNOLOGY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410707566.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

The polyurethane outer sheath of the charging pile cable is easily broken due to frequent bending during use, damaging the internal structure of the cable and shortening the cable life.

Method used

Using modified polyurethane matrix material, by adding white carbon black, nano-calcium carbonate, nano-titanium dioxide, pentaerythritol, nano-magnesium hydroxide and other ingredients, combined with elastic particles and elastic fibers, the bending resistance and mechanical properties of the material are enhanced to form a flexible, Wear-resistant and anti-aging outer sheath.

Benefits of technology

It significantly improves the bending resistance, abrasion resistance and weather resistance of the cable outer sheath, extending the service life of the cable. Through the combination of elastic particles and fibers, it disperses and transfers stress and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the field of charging pile cable materials, a polyurethane material for charging pile cables, including the following raw materials in parts by weight: modified polyurethane matrix material, white carbon black, nano calcium carbonate, coupling agent, nano titanium dioxide, pentaerythritol, nano magnesium hydroxide, paraffin oil, elastic particles, elastic fibers; the preparation of the modified polyurethane matrix material includes the following steps: S1: polycarbonate diol, isophorone diisocyanate, acetone and 1,4-butanediol are used as raw materials to prepare a polyurethane prepolymer; S2: the polyurethane prepolymer prepared in step S1 is mixed with vinyl triethoxysilane and hexafluorobutyl methacrylate at room temperature, and reacted to obtain a modified polyurethane matrix material. The polyurethane material prepared in the present application has good bending resistance, weather resistance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of charging pile cable materials, and more specifically, it relates to a polyurethane material for charging pile cables. Background Art

[0002] With the rapid development of new energy vehicles, charging piles are also widely used. Charging piles can charge various models of electric vehicles according to different voltage levels. The basic structure of the power cable of the charging pile consists of four parts: core (conductor), insulation layer, shielding layer and outer sheath. The core is the conductive part of the power cable, which is used to transmit electric energy and is the main part of the power cable. The insulation layer electrically isolates the core from the earth and the cores of different phases from each other to ensure the transmission of electric energy. The outer sheath is an indispensable component of the power cable structure. Its function is to protect the power cable from the intrusion of external impurities and moisture, and to prevent external forces from directly damaging the power cable.

[0003] As an emerging polymer material with broad development prospects, polyurethane has excellent comprehensive performance and wide applications, and is known as the "fifth plastic". Thermoplastic polyurethane elastomer (TPU) has two functional raw materials for synthesis, so there is basically no chemical cross-linking between its molecular chains. Therefore, its processing performance, mechanical properties and low-temperature performance are very outstanding, so it is often used as the outer sheath material of cables.

[0004] In actual use, due to the frequent use of charging piles, the cables are often bent during use, which makes the polyurethane outer sheath easy to rupture, thereby damaging the internal structure of the cable and shortening the cable life. Summary of the invention

[0005] In order to improve the bending resistance of the outer sheath of a charging pile cable, the present application provides a polyurethane material for a charging pile cable.

[0006] The present application provides a polyurethane material for a charging pile cable, which adopts the following technical solution:

[0007] A polyurethane material for a charging pile cable, comprising the following raw materials in parts by weight: 80-100 parts of a modified polyurethane matrix material, 6-7 parts of white carbon black, 4-6 parts of nano calcium carbonate, 0.5-1 parts of a coupling agent, 3-4 parts of nano titanium dioxide, 5-6 parts of pentaerythritol, 3-4 parts of nano magnesium hydroxide, 1-2 parts of paraffin oil, 18-25 parts of elastic particles, and 20-24 parts of elastic fibers;

[0008] The preparation of the modified polyurethane matrix material comprises the following steps:

[0009] S1: First, at a temperature of 100-110°C and a rotation speed of 300-350r / min, 20-22 parts by weight of polycarbonate diol are stirred while vacuuming for 30-35 minutes, and then cooled. When the temperature drops to 50-55°C, 22-23 parts by weight of isophorone diisocyanate, 15-18 parts by weight of acetone and 5-8 parts by weight of 1,4-butanediol are added to the polycarbonate diol, mixed, and stirred while vacuuming. After stirring evenly, the temperature is raised to 75-85°C, and the reaction is kept at this temperature for 0.8-1.0h to obtain a polyurethane prepolymer;

[0010] S2: mixing the polyurethane prepolymer prepared in step S1 with 5-8 parts by weight of vinyl triethoxysilane and 25-30 parts by weight of hexafluorobutyl methacrylate at room temperature, and reflux reacting at 60-70° C. for 2-4 hours to obtain a modified polyurethane matrix material;

[0011] The preparation of the elastic fiber comprises the following steps:

[0012] S1: 12-20 parts by weight of polyacrylate emulsion, 2-3 parts by weight of nano-silicon dioxide, 1.2-1.5 parts by weight of toughening agent, 0.1-0.15 parts by weight of curing agent and 0.5-0.8 parts by weight of coupling agent are mixed at room temperature to form a modifier;

[0013] S2: immersing 10-15 parts by weight of glass fiber in the modifier for 10-15 minutes, taking it out, and curing it at 80-100° C. for 1-2 hours to obtain elastic fiber;

[0014] The preparation of the elastic particles comprises the following steps:

[0015] 20-25 parts by weight of polyether polyol, 25-40 parts by weight of diphenylmethane diisocyanate, 22-28 parts by weight of polytetrahydrofuran diol and 3-5 parts by weight of sepiolite powder are uniformly mixed at room temperature, reacted at 70-85° C. for 50-100 min, and reacted at 70-85° C. for 50-100 min to obtain a mixture, and the mixture is added into a single-screw granulator for granulation, the screw speed is 160-180 rpm, the extrusion temperature is 180-240° C., and the elastic particles are obtained after cooling at room temperature for 5-6 hours.

[0016] By adopting the above technical solution, the modified polyurethane matrix material in the present application is a fluorosilicone modified polyurethane matrix material, which increases the flexibility, bending resistance, wear resistance and weather resistance of the cable sheath, thereby extending the service life of the cable;

[0017] The modified polyurethane matrix material prepared in the present application also contains nano titanium dioxide to increase the anti-aging performance of the polyurethane matrix material. The pentaerythritol in the present application increases the flexibility of the urethane matrix material, thereby increasing the bending resistance of the polyurethane matrix material. The nano magnesium hydroxide in the present application increases the flame retardancy of the polyurethane matrix material. The white carbon black and nano calcium carbonate in the present application increase the mechanical properties of the polyurethane matrix material. The coupling agent in the present application increases the compatibility of each component, thereby improving the comprehensive performance of the polyurethane matrix material.

[0018] The modified polyurethane matrix material prepared in the present application also includes elastic particles and elastic fibers, which can increase the elasticity, impact resistance, and fatigue resistance of the polyurethane matrix material, thereby improving the bending resistance of the polyurethane material. In addition, the present application uses elastic particles and elastic fibers in combination. On the one hand, when stress is applied to the outer sheath of the cable, the elastic fibers can absorb and disperse the stress, while the elastic particles can transfer the stress from the surface of the material to the inside of the material, thereby reducing the stress concentration on the surface of the material and improving the bending resistance and durability of the material; on the other hand, the elastic particles have a small molecular weight and good fluidity, and can be distributed more evenly in the polyurethane system, which is beneficial to improving the bending resistance of the polyurethane material. Although the fluidity of elastic fibers is worse than that of elastic fibers, elastic fibers can have higher tensile strength and elongation at break due to the long molecular chain and stronger intermolecular forces, which means that the outer sheath of the cable has a greater ability to resist deformation and fracture when subjected to tensile stress. Therefore, the elastic particles and elastic fibers in the present application are used in combination with each other, and their functions are complementary, which can effectively improve the bending resistance and mechanical properties of the outer sheath of the cable;

[0019] In summary, the present application performs fluorine-silicon modification on the polyurethane material, which can effectively improve the mechanical properties, bending resistance and wear resistance of the polyurethane material. The present application also uses a variety of substances such as nano-titanium dioxide, pentaerythritol, sodium magnesium hydroxide, and white carbon black to improve the comprehensive performance of the polyurethane material. The present application uses elastic particles and elastic fibers in combination with each other, with complementary functions, which can effectively improve the bending resistance and mechanical properties of the polyurethane material.

[0020] The glass fiber in the present application has high strength and can effectively improve the strength of the cable outer sheath. The present application adopts polyacrylic acid emulsion to modify the glass fiber. The polyacrylic acid emulsion can form a soft polymer layer on the surface of the glass fiber, forming a special soft-hard core-shell structure, which can effectively promote stress dispersion, avoid stress concentration, and achieve the function of strengthening and toughening the glass fiber, thereby improving the bending resistance and mechanical properties of the polyurethane material;

[0021] The present application also uses nano-silicon dioxide elastic fibers to enhance the roughness of the elastic fiber surface, thereby enhancing the bonding force between the elastic fiber and the polyurethane material.

[0022] The elastic particles prepared by the above-mentioned preparation method in the present application have good elasticity. The present application also incorporates sepiolite into the elastic particles. When the elastic particles are directly impacted by the outside world, they can be buffered by the elastic displacement and resetting of the sepiolite, thereby improving the elastic effect of the elastomer. In addition, since the pore size of sepiolite is large and abundant, it can further attenuate the stress received, thereby further improving the bending resistance of the polyurethane material.

[0023] Preferably, the mass ratio of the elastic particles to the elastic fibers is (19-20): (22-23).

[0024] By adopting the above technical solution, when the mass ratio of elastic particles to elastic fibers is (19-20): (22-23), the two can further cooperate to improve the bending resistance and mechanical properties of the polyurethane material.

[0025] Preferably, the particle size of the elastic particles is 100-500 µm, the length of the elastic fibers is 1-5 mm, and the diameter of the elastic fibers is 20-30 µm.

[0026] By adopting the above technical solution, when the elastic particles and the elastic fibers are of the above sizes, the two can further cooperate with each other to improve the bending resistance and mechanical properties of the polyurethane material.

[0027] Preferably, the elastic particles are formed by mixing elastic particles with a particle size of 100-150µm, elastic particles with a particle size of 220-280µm and elastic particles with a particle size of 380-500µm. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 280-340r / min. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 130-180r / min. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 70-100r / min.

[0028] Preferably, the weight ratio of the 100-150 µm elastic particles, the 220-280 µm elastic particles and the 380-500 µm elastic particles is 1:1.2:1.5.

[0029] By adopting the above technical solution, when the particle size of the elastic particles is the above gradation, the outer sheath of the manufactured cable has good bending resistance and mechanical properties.

[0030] Preferably, the particle size of the sepiolite powder is 10-20 μm.

[0031] By adopting the above technical solution, if the particle size of the sepiolite powder is too small, it is easy to agglomerate, and if the particle size of the sepiolite powder is too large, the binding force with the matrix polymer is weak.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. The present application performs fluorine-silicon modification on the polyurethane material, which can effectively improve the mechanical properties, bending resistance and wear resistance of the cable outer sheath. The present application also uses a variety of substances such as nano-titanium dioxide, pentaerythritol, sodium magnesium hydroxide, and white carbon black to improve the comprehensive performance of the outer sheath. The present application uses elastic particles and elastic fibers in combination with each other, which have complementary functions and can effectively improve the bending resistance and mechanical properties of the cable outer sheath.

[0034] 2. The elastic particles prepared by the above-mentioned preparation method in the present application have good elasticity. The present application also incorporates sepiolite into the elastic particles. When the elastic particles are directly impacted by the outside world, they can be buffered by the elastic displacement and resetting of the sepiolite, thereby improving the elastic effect of the elastomer. In addition, since the pore size of sepiolite is large and abundant, it can further attenuate the stress received, thereby further improving the bending resistance of the polyurethane material.

[0035] 3. Glass fiber has high strength and can effectively improve the strength of the cable outer sheath. This application uses polyacrylic acid emulsion to modify the glass fiber. The polyacrylic acid emulsion can form a soft polymer layer on the surface of the glass fiber, forming a special soft-hard core-shell structure, which can effectively promote stress dispersion, avoid stress concentration, and achieve the function of strengthening and toughening the glass fiber, thereby improving the bending resistance and mechanical properties of the cable outer sheath.

[0036] Source of raw materials:

[0037] Polycarbonate diol was from Hubei Wonder Chemical Co., Ltd., model WD03658;

[0038] Isophorone diisocyanate was from Hubei Zhenbo Chemical Co., Ltd., with a purity of 99%;

[0039] Vinyltriethoxysilane was from Jining Hongming Chemical Reagent Co., Ltd., model A-151;

[0040] Hexafluorobutyl methacrylate was from Shaoguan Keya Fine Chemical Co., Ltd., product number GA651423;

[0041] Polyacrylate emulsion was from Jinan Tuoda Building Materials Co., Ltd., item number 00041;

[0042] The toughening agent is nitrile rubber powder, which comes from Tuoyi New Materials Co., Ltd.

[0043] The curing agent was from Shanghai Motian Chemical Co., Ltd., model WAT-4;

[0044] Polyether polyol was from Jining Hongming Chemical Reagent Co., Ltd., model 403;

[0045] Diphenylmethane diisocyanate was from Hubei Xinrunde Chemical Co., Ltd.;

[0046] Polytetrahydrofurandiol was obtained from Guangdong Wengjiang Chemical Reagent Co., Ltd., product number PTMEG;

[0047] Sepiolite powder comes from Lingshou County Hongchang Mineral Products Processing Plant;

[0048] KH580 coupling agent comes from Henan Chunqi Chemical Co., Ltd.;

[0049] The glass fiber comes from Taian Jiacheng Fiber Co., Ltd. DETAILED DESCRIPTION

[0050] The present application is further described in detail below in conjunction with preparation examples and embodiments.

[0051] Preparation Example

[0052] Preparation of modified polyurethane matrix materials

[0053] Preparation Example 1.1

[0054] The preparation of the modified polyurethane matrix material comprises the following steps:

[0055] S1: First, at a temperature of 100°C and a rotation speed of 300r / min, 20kg of polycarbonate diol was stirred while vacuuming for 30min, and then cooled. When the temperature dropped to 50°C, 22kg of isophorone diisocyanate, 15kg of acetone and 5kg of 1,4-butanediol were added to the polycarbonate diol and mixed, and the mixture was stirred while vacuuming. After stirring evenly, when the temperature rose to 75°C, the mixture was kept warm for 0.8h to obtain a polyurethane prepolymer.

[0056] S2: The polyurethane prepolymer prepared in step S1 is mixed with 5 kg of vinyl triethoxysilane and 25 kg of hexafluorobutyl methacrylate at room temperature, and refluxed at 60° C. for 2 h to obtain a modified polyurethane matrix material.

[0057] Preparation Example 1.2

[0058] The preparation of the modified polyurethane matrix material comprises the following steps:

[0059] S1: First, at a temperature of 105°C and a rotation speed of 320r / min, 21kg of polycarbonate diol was stirred while vacuuming for 32 minutes, and then cooled. When the temperature dropped to 52°C, 22.5kg of isophorone diisocyanate, 16kg of acetone and 7kg of 1,4-butanediol were added to the polycarbonate diol and mixed, and the mixture was stirred while vacuuming. After stirring evenly, the temperature was raised to 80°C, and the mixture was kept warm for 0.9h to obtain a polyurethane prepolymer;

[0060] S2: The polyurethane prepolymer prepared in step S1 was mixed with 6 kg of vinyl triethoxysilane and 27 kg of hexafluorobutyl methacrylate at room temperature, and refluxed at 65° C. for 3 h to obtain a modified polyurethane matrix material.

[0061] Preparation Example 1.3

[0062] The preparation of the modified polyurethane matrix material comprises the following steps:

[0063] S1: First, at a temperature of 110°C and a rotation speed of 350r / min, 22kg of polycarbonate diol was stirred while vacuuming for 35min, and then cooled. When the temperature dropped to 55°C, 23kg of isophorone diisocyanate, 18kg of acetone and 8kg of 1,4-butanediol were added to the polycarbonate diol and mixed, and the mixture was stirred while vacuuming. After stirring evenly, the mixture was kept warm for 1h to obtain a polyurethane prepolymer.

[0064] S2: The polyurethane prepolymer prepared in step S1 was mixed with 8 kg of vinyl triethoxysilane and 30 kg of hexafluorobutyl methacrylate at room temperature, and refluxed at 70° C. for 4 hours to obtain a modified polyurethane matrix material.

[0065] Preparation of elastic fibers

[0066] Preparation Example 2.1

[0067] The preparation of elastic fiber comprises the following steps:

[0068] S1: 12kg polyacrylate emulsion, 2kg nano-silicon dioxide, 1.2kg toughening agent, 0.1kg curing agent and 0.5kg KH-560 coupling agent were mixed at room temperature to form a modifier;

[0069] S2: 10 kg of glass fiber is immersed in the modifier for 10 minutes, taken out, and cured at 80° C. for 1 hour to obtain elastic fiber; the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 μm.

[0070] Preparation Example 2.2

[0071] The preparation of elastic fiber comprises the following steps:

[0072] S1: 16 kg polyacrylate emulsion, 2.5 kg nano-silicon dioxide, 1.3 kg toughening agent, 0.12 kg curing agent and 0.6 kg KH-560 coupling agent were mixed at room temperature to form a modifier;

[0073] S2: 12 kg of glass fiber is immersed in the modifier for 12 minutes, taken out, and cured at 90° C. for 1.5 hours to obtain elastic fiber; the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 μm.

[0074] Preparation Example 2.3

[0075] The preparation of elastic fiber comprises the following steps:

[0076] S1: 20kg polyacrylate emulsion, 3kg nano-silicon dioxide, 1.5kg toughening agent, 0.15kg curing agent and 0.8kg KH-560 coupling agent were mixed at room temperature to form a modifier;

[0077] S2: 15 kg of glass fiber is immersed in the modifier for 15 minutes, taken out, and cured at 100° C. for 2 hours to obtain elastic fiber; the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 μm.

[0078] Preparation of elastic particles

[0079] Preparation Example 3.1

[0080] The preparation of elastic particles includes the following steps:

[0081] 20 kg of polyether polyol, 25 kg of diphenylmethane diisocyanate, 22 kg of polytetrahydrofuran diol and 3 kg of sepiolite powder were mixed uniformly at room temperature, reacted at 70° C. for 50 min to obtain a mixture, and the mixture was added into a single screw granulator for granulation, the screw speed was 160 rpm, the extrusion temperature was 240° C., the feeding speed was 30 kg / h, the pelletizing speed was 280-340 r / min, and after cooling at room temperature for 5 h, elastic particles with a particle size of 100-150 μm were obtained;

[0082] Among them, the particle size of sepiolite powder is 10-20µm.

[0083] Preparation Example 3.2

[0084] The preparation of elastic particles includes the following steps:

[0085] 22 kg of polyether polyol, 34 kg of diphenylmethane diisocyanate, 25 kg of polytetrahydrofuran diol and 4 kg of sepiolite powder were mixed uniformly at room temperature, reacted at 78° C. for 70 min to obtain a mixture, and the mixture was added into a single screw granulator for granulation, the screw speed was 180 rpm, the extrusion temperature was 180° C., the feeding speed was 30 kg / h, the pelletizing speed was 280-340 r / min, and after cooling at room temperature for 5 h, elastic particles with a particle size of 100-150 μm were obtained;

[0086] Among them, the particle size of sepiolite powder is 10-20µm.

[0087] Preparation Example 3.3

[0088] The preparation of elastic particles includes the following steps:

[0089] 25 kg of polyether polyol, 40 kg of diphenylmethane diisocyanate, 28 kg of polytetrahydrofuran diol and 5 kg of sepiolite powder were mixed uniformly at room temperature, reacted at 85° C. for 100 min to obtain a mixture, and the mixture was added into a single screw granulator for granulation at a screw speed of 170 rpm, an extrusion temperature of 200° C., a feeding speed of 30 kg / h, a pelletizing speed of 280-340 r / min, and cooled at room temperature for 6 h to obtain elastic particles with a particle size of 100-150 μm;

[0090] Among them, the particle size of sepiolite powder is 10-20µm.

[0091] Preparation Example 3.4

[0092] The difference between Preparation Example 3.4 and Preparation Example 3.3 is that the particle size of the sepiolite powder is 20-50µm, and the remaining steps are the same as Preparation Example 3.3.

[0093] Preparation Example 3.5

[0094] The difference between Preparation Example 3.5 and Preparation Example 3.2 is that the cutting speed of the single-screw granulator is adjusted to 130-180r / min, and the particle size of the obtained elastic particles is 220-280µm. The remaining steps are the same as Preparation Example 3.2.

[0095] Preparation Example 3.6

[0096] The difference between Preparation Example 3.6 and Preparation Example 3.2 is that the cutting speed of the single-screw granulator is adjusted to 70-100 r / min, and the particle size of the obtained elastic particles is 380-500 µm. The remaining steps are the same as Preparation Example 3.2.

[0097] Example

[0098] The following are examples of the present application.

[0099] Example 1

[0100] A polyurethane material for a charging pile cable includes the following preparation method:

[0101] S1: 80 kg of modified polyurethane matrix material, 6 kg of white carbon black, 4 kg of nano calcium carbonate, 0.5 kg of KH-580 coupling agent, 3 kg of nano titanium dioxide, 5 kg of pentaerythritol, 3 kg of nano magnesium hydroxide, 1 kg of paraffin oil, 18 kg of elastic particles and 20 kg of elastic fiber were weighed and put into an open mill, heated to above 75° C., and stirred and mixed for 30-50 minutes to obtain a premix;

[0102] Step S2: The premix is ​​put into a twin-screw extruder for melt blending and extrusion, and after pulling, cooling and drying, a polyurethane material for a charging pile cable is obtained.

[0103] Wherein, the modified polyurethane matrix material comes from Preparation Example 1.1, the elastic fiber comes from Preparation Example 2.1, the elastic particles come from Preparation Example 3.1, the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 µm.

[0104] Example 2

[0105] A polyurethane material for a charging pile cable includes the following preparation method:

[0106] S1: 90 kg of modified polyurethane matrix material, 6.5 kg of white carbon black, 5 kg of nano calcium carbonate, 0.7 kg of KH-580 coupling agent, 3.5 kg of nano titanium dioxide, 5.5 kg of pentaerythritol, 3.5 kg of nano magnesium hydroxide, 1.5 kg of paraffin oil, 22 kg of elastic particles and 22 kg of elastic fiber were weighed and put into an open mill, heated to above 75° C., stirred and mixed for 30-50 min to obtain a premix;

[0107] Step S2: The premix is ​​put into a twin-screw extruder for melt blending and extrusion, and after pulling, cooling and drying, a polyurethane material for a charging pile cable is obtained.

[0108] Among them, the modified polyurethane matrix material comes from Preparation Example 1.2, the elastic fiber comes from Preparation Example 2.2, the elastic particles come from Preparation Example 3.2, the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 µm.

[0109] Example 3

[0110] A polyurethane material for a charging pile cable includes the following preparation method:

[0111] S1: Weigh 100 kg of modified polyurethane matrix material, 7 kg of white carbon black, 6 kg of nano calcium carbonate, 1 kg of KH-580 coupling agent, 4 kg of nano titanium dioxide, 6 kg of pentaerythritol, 4 kg of nano magnesium hydroxide, 2 kg of paraffin oil, 25 kg of elastic particles and 24 kg of elastic fiber into an open mill, heat to above 75° C., stir and mix for 30-50 minutes to obtain a premix;

[0112] Step S2: The premix is ​​put into a twin-screw extruder for melt blending and extrusion, and after pulling, cooling and drying, a polyurethane material for a charging pile cable is obtained.

[0113] Among them, the modified polyurethane matrix material comes from Preparation Example 1.3, the elastic fiber comes from Preparation Example 2.3, the elastic particles come from Preparation Example 3.3, the length of the elastic fiber is 1-5 mm, and the diameter of the elastic fiber is 20-30 µm.

[0114] Embodiment 4-8

[0115] The difference between Example 4-8 and Example 2 is that the mass and mass ratio of the elastic particles and the elastic fibers are different. The specific data are shown in the following table:

[0116]

[0117] Example 9

[0118] The difference between Example 9 and Example 5 is that the elastic particles come from Preparation Example 3.5, and the remaining steps are the same as Example 5.

[0119] Example 10

[0120] The difference between Example 10 and Example 5 is that the elastic particles come from Preparation Example 3.6, and the remaining steps are the same as Example 5.

[0121] Examples 11-14

[0122] The difference between Examples 11-14 and Example 5 is that the elastic particles are prepared by mixing the elastic particles from Preparation Example 3.3, the elastic particles from Preparation Example 3.5 and the elastic particles from Preparation Example 3.6. The total amount of the elastic particles from the above three preparation examples mixed together is 22 kg, and the weight to weight ratio of the 100-150 µm elastic particles (from Preparation Example 3.3), the 220-280 µm elastic particles (from Preparation Example 3.5) and the 380-500 µm elastic particles (from Preparation Example 3.6) is different, as shown in the following table:

[0123] Table 2 The mass and mass ratio of elastic particles of different particle sizes in Examples 11-14

[0124]

[0125] Embodiment 15

[0126] The difference between Example 15 and Example 13 is that the elastic particles with a particle size of 100-150 μm come from Preparation Example 3.4, and the remaining steps are the same as Example 13.

[0127] Example 16

[0128] The difference between Example 16 and Example 13 is that the elastic fiber is prepared using the method of Preparation Example 3.2, the length of the elastic fiber is 5-7 mm, the diameter of the elastic fiber is 20-30 µm, and the remaining steps are the same as Example 13.

[0129] Comparative Example

[0130] The following is a comparative example of the present application.

[0131] Comparative Example 1

[0132] The difference between Comparative Example 1 and Example 1 is that the S2 fluorosilicone modification step is not performed during the preparation of the polyurethane material, and the remaining steps are the same as those in Example 1.

[0133] Comparative Example 2

[0134] The difference between Comparative Example 2 and Example 1 is that the elastic particles are replaced with an equal amount of elastic fibers, and the remaining steps are the same as those of Example 1.

[0135] Comparative Example 3

[0136] The difference between Comparative Example 3 and Example 1 is that the elastic fibers are replaced with an equal amount of elastic particles, and the remaining steps are the same as those of Example 1.

[0137] Comparative Example 4

[0138] The difference between Comparative Example 4 and Example 1 is that, in the process of preparing elastic particles by the preparation method of Preparation Example 3.1, the sepiolite powder is replaced by an equal amount of silicon dioxide with an equal particle size to obtain elastic particles, and the remaining steps are the same as in Example 1.

[0139] Performance testing

[0140] Detection Methods

[0141] Anti-bending performance test: A bending test machine was used to conduct anti-bending performance swing test on the polyurethane materials prepared in Examples 1-16 and Comparative Examples 1-4. The polyurethane material was made to be 3mm thick, and a weight was added as a load so that the applied force was 5N. A clamping plate R=10mm swing mechanism was used to swing 180° (90° on both sides of the plumb line), the number of swings was 5000, and the swing rate was 30 times per minute. The polyurethane materials prepared in each example and comparative example were set to 50 groups, and the 50 groups of polyurethane materials were subjected to anti-bending performance swing test, and the number of polyurethane materials that were broken or cracked was counted;

[0142] Tensile property test: The tensile strength test of the polyurethane materials prepared in Examples 1-16 and Comparative Examples 1-4 was performed according to the tensile strength test in the national standard GB / T 528-1998 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber";

[0143] Weather resistance test: Refer to the experimental method in GB / T 16422.2-2014 "Plastic Laboratory Light Source Exposure Test Method Part 2: Xenon Arc Lamp" to conduct weather resistance tests on the polyurethane materials prepared in Examples 1-16 and Comparative Examples 1-4, and score them. Experimental instruments: xenon arc lamp, test chamber (humidity control in accordance with ISO 4892-1), irradiator (in accordance with ISO4892-1). Scoring criteria: If there are no cracks, discoloration, or damage on the surface of the polyurethane material, it is recorded as '0'; if there are cracks, discoloration, or other problems on the surface, it is recorded as '1'; the specific test results are shown in the following table:

[0144]

[0145] Combining the data of Examples 1-3 and Table 3, it can be seen that the polyurethane materials prepared in Examples 1-3 of the present application have a pass rate of 92% after the bending resistance test, and the tensile strength reaches 17 MPa. After the weathering test, there is no crack, no discoloration, and no damage on the surface of the polyurethane material.

[0146] Combining the data of Example 2, Examples 4-8 and Table 3, it can be seen that when the mass ratio of elastic particles to elastic fibers is (19-20): (22-23), the two can further play a cooperative role to improve the bending resistance and mechanical properties of the polyurethane material.

[0147] From the data of Example 5, Examples 9-14 and Table 3, it can be seen that adjusting the particle size of the elastic particles and grading the 100-150µm elastic particles, the 220-280µm elastic particles and the 380-500µm elastic particles can effectively improve the bending resistance of the polyurethane material, and when the weight ratio of the 100-150µm elastic particles, the 220-280µm elastic particles and the 380-500µm elastic particles is 1:1.2:1.5, the prepared polyurethane material has good bending resistance and mechanical properties.

[0148] Combining the data of Example 13 and Example 15 and Table 3, it can be seen that the sepiolite powder with a particle size of 10-20µm can adapt to 100-150µm elastic particles, 220-280µm elastic particles and 380-500µm elastic particles.

[0149] Combining the data of Example 13, Example 16 and Table 3, it can be seen that when the length of the elastic fiber is 1-5 mm, it can cooperate well with the elastic particles of the above particle size, and the two can further play a cooperative role to improve the bending resistance and mechanical properties of the cable outer sheath.

[0150] Combining the data of Comparative Example 1, Example 1 and Table 3, it can be seen that the polyurethane material in the present application is modified with fluorine and silicon, which increases the flexibility, bending resistance, wear resistance and weather resistance of the cable sheath, thereby extending the service life of the cable.

[0151] Combining the data of Example 1, Comparative Examples 2-3 and Table 3, it can be seen that the elastic particles and elastic fibers are used in combination with each other, and their functions are complementary, which can effectively improve the bending resistance and mechanical properties of the cable outer sheath.

[0152] Combining the data of Example 1, Comparative Example 4 and Table 3, it can be seen that by adding sepiolite powder during the preparation of elastic particles and filling the prepared elastic particles into the cable outer sheath, the bending resistance of the cable outer sheath can be effectively improved.

[0153] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A polyurethane material for charging pile cables, characterized in that: The invention comprises the following raw materials in parts by weight: 80-100 parts of modified polyurethane matrix material, 6-7 parts of white carbon black, 4-6 parts of nano calcium carbonate, 0.5-1 parts of coupling agent, 3-4 parts of nano titanium dioxide, 5-6 parts of pentaerythritol, 3-4 parts of nano magnesium hydroxide, 1-2 parts of paraffin oil, 18-25 parts of elastic particles, and 20-24 parts of elastic fiber; The preparation of the modified polyurethane matrix material comprises the following steps: S1: First, at a temperature of 100-110°C and a rotation speed of 300-350r / min, 20-22 parts by weight of polycarbonate diol are stirred while vacuuming for 30-35 minutes, and then cooled. When the temperature drops to 50-55°C, 22-23 parts by weight of isophorone diisocyanate, 15-18 parts by weight of acetone and 5-8 parts by weight of 1,4-butanediol are added to the polycarbonate diol, mixed, and stirred while vacuuming. After stirring evenly, the temperature is raised to 75-85°C, and the reaction is kept at this temperature for 0.8-1.0h to obtain a polyurethane prepolymer; S2: mixing the polyurethane prepolymer prepared in step S1 with 5-8 parts by weight of vinyl triethoxysilane and 25-30 parts by weight of hexafluorobutyl methacrylate at room temperature, and reflux reacting at 60-70° C. for 2-4 hours to obtain a modified polyurethane matrix material; The preparation of the elastic fiber comprises the following steps: S1: 12-20 parts by weight of polyacrylate emulsion, 2-3 parts by weight of nano-silicon dioxide, 1.2-1.5 parts by weight of toughening agent, 0.1-0.15 parts by weight of curing agent and 0.5-0.8 parts by weight of coupling agent are mixed at room temperature to form a modifier; S2: immersing 10-15 parts by weight of glass fiber in the modifier for 10-15 minutes, taking it out, and curing it at a temperature of 80-100° C. for 1-2 hours to obtain elastic fiber; The preparation of the elastic particles comprises the following steps: 20-25 parts by weight of polyether polyol, 25-40 parts by weight of diphenylmethane diisocyanate, 22-28 parts by weight of polytetrahydrofuran diol and 3-5 parts by weight of sepiolite powder are uniformly mixed at room temperature, reacted at 70-85° C. for 50-100 minutes to obtain a mixture, and the mixture is added into a single-screw granulator for granulation at a screw speed of 160-180 rpm and an extrusion temperature of 180-240° C. The elastic particles are obtained after cooling at room temperature for 5-6 hours.

2. The polyurethane material for charging pile cables according to claim 1, characterized in that: The mass ratio of the elastic particles to the elastic fibers is (19-20): (22-23).

3. The polyurethane material for charging pile cables according to claim 2, characterized in that: The particle size of the elastic particles is 100-500 μm, the length of the elastic fibers is 1-5 mm, and the diameter of the elastic fibers is 20-30 μm.

4. The polyurethane material for charging pile cables according to claim 3, characterized in that: The elastic particles are prepared by mixing elastic particles with a particle size of 100-150µm, elastic particles with a particle size of 220-280µm and elastic particles with a particle size of 380-500µm. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 280-340r / min. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 130-180r / min. During the preparation of the elastic particles with a particle size of 100-150µm, the feeding speed of the single screw granulator is 30kg / h, and the pelletizing speed is 70-100r / min.

5. The polyurethane material for charging pile cables according to claim 4, characterized in that: The weight ratio of the 100-150µm elastic particles, the 220-280µm elastic particles and the 380-500µm elastic particles is 1:1.2:1.

5.

6. The polyurethane material for charging pile cables according to claim 1, characterized in that: The particle size of the sepiolite powder is 10-20 μm.

Citation Information

Patent Citations

  • High-thermal-conductivity insulating rubber material for cable of electric vehicle charging pile and preparation method of high-thermal-conductivity insulating rubber material

    CN108384125A

  • High elasticity HDPE resin and preparation method thereof

    CN108752680A

  • Marine flame-retardant corrosion-resistant polyurethane cable sheath material

    CN108841162A

  • Nano in-situ fiber-forming elastomer fiber toughened polymer material

    CN111718544A

  • Production process of high-performance halogen-free polyurethane flame-retardant cable sheath material

    CN115558278A