A pressure-sensitive adhesive resin composition with low skin sensitivity and a method for preparing a pressure-sensitive adhesive tape

Through the composition of high-purity polyacrylic resin and tackifying resin, the conversion rate of VOC and monomer is controlled, and the sensitivity and residual glue problems of pressure-sensitive adhesive during skin bonding are solved, achieving efficient skin-friendliness and transparency sex.

CN118291062BActive Publication Date: 2024-11-22QINGYUAN HUMAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410401227.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-11-22
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesives have high sensitivity when skin bonding. When removed, there are many residual adhesives that irritate the skin and reduce adhesion. Especially in the medical field, there are high requirements for transparency.

Method used

The composition of 50~98 wt% polyacrylic resin, 0~50 wt% tackifying resin and 0.01~2 wt% curing agent is used to control the VOC content below 500 ppm, the monomer conversion rate exceeds 99%, and high-purity monomer and female Water monomer, reasonably formulate soft and hard monomers to reduce skin sensitivity.

Benefits of technology

It achieves low skin sensitivity, reduces residual glue, improves adhesion and transparency, and reduces irritation to the skin. It is suitable for long-term skin adhesion applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a low skin sensitivity pressure-sensitive adhesive resin composition and a method for preparing a pressure-sensitive adhesive tape, wherein the pressure-sensitive adhesive resin composition is composed of 50-98wt% polyacrylic acid resin, 0-50wt% tackifying resin and 0.01-2wt% curing agent, the VOC content of the pressure-sensitive adhesive resin composition is controlled below 500ppm, and the monomer conversion rate exceeds 99%. The pressure-sensitive adhesive tape prepared by the present invention has low skin sensitivity, no abnormality and no residual adhesive after a 4-hour skin test, and has good air permeability and low sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of acrylic resin adhesives, and in particular relates to a pressure-sensitive adhesive resin composition with low skin sensitivity and a method for preparing a pressure-sensitive adhesive tape. Background Art

[0002] Pressure-sensitive adhesive is a viscoelastic material that can adhere to the surface of the adherend in a short time by applying a slight contact pressure. At present, pressure-sensitive adhesive products are widely used in packaging, construction, communications, automobiles, medical and health care, and home care industries. Among them, with the development of medical treatment and medical devices, pressure-sensitive adhesives for human skin also pose new challenges. The requirements for this type of pressure-sensitive adhesive are: good adhesion to the skin, no residual adhesive when removed and no skin damage, no obvious decrease in adhesion during bonding and no irritation to the skin, and even some medical devices require high transparency. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention provides a low skin sensitivity pressure-sensitive adhesive resin composition and a method for preparing a pressure-sensitive adhesive tape, which reduce the content of impurities in the resin and reduce or avoid the use of irritating monomers, thereby reducing skin sensitivity.

[0004] In order to solve the above technical problems, the present invention adopts the following technical scheme: a pressure-sensitive adhesive resin composition with low skin sensitivity, which is composed of 50~98wt% of polyacrylic resin, 0~50wt% of tackifying resin and 0.01~2wt% of curing agent, the VOC content of the pressure-sensitive adhesive resin composition is controlled below 500ppm, and the conversion rate of each monomer exceeds 99%.

[0005] Preferably, the polyacrylic acid resin is polymerized by reactive monomers under the action of an initiator, and the reactive monomers include soft monomers, hard monomers and functional monomers; and the reactive monomers of the polyacrylic acid resin include at least one hydrophilic monomer.

[0006] Preferably, the purity of the raw materials of the pressure-sensitive adhesive resin composition is above 98%, and the content of carcinogens and allergens in the raw materials accounts for less than 0.1% of the total weight of the pressure-sensitive adhesive resin composition.

[0007] Preferably, the soft monomer includes one or more of methyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, isodecyl acrylate, lauryl methacrylate, lauryl acrylate, and dodecyl acrylate.

[0008] Preferably, the hard monomer includes one or more of methyl methacrylate, ethyl methacrylate, isobutyl methacrylate or isobornyl methacrylate.

[0009] Preferably, the functional monomer includes one or more of 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, and hydroxybutyl acrylate.

[0010] Preferably, the thermal initiator is azobisisobutyronitrile or benzoyl peroxide; the tackifying resin is rosin resin or terpene resin; and the curing agent model is N3390.

[0011] Preferably, the hydrophilic monomer is one or more of methyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, and hydroxybutyl acrylate, and the weight percentage of the hydrophilic monomer is ≥5% of the content of the reactive monomer.

[0012] The present invention also provides a method for preparing a pressure-sensitive adhesive tape based on the pressure-sensitive adhesive resin composition with low skin sensitivity, comprising the following steps:

[0013] S1, preparation of polyacrylic acid resin: soft monomer, hard monomer, functional monomer and initiator are uniformly mixed according to mass ratio to obtain a mixture of monomer and initiator; a proper amount of solvent ethyl acetate is added into a reaction kettle, and nitrogen is flushed in to deoxygenate for at least 1 hour, the system is heated to 70±3° C., and the mixture of monomer and initiator is slowly dripped into the reaction kettle within 2-5 hours, and the mixture is kept warm for polymerization reaction for 3-5 hours, and the reaction is stopped when the monomer conversion rate reaches more than 99% to obtain a polyacrylic acid resin with a viscosity of 3000-7000 mPa·s;

[0014] S2, mixing the polyacrylic acid resin obtained in step S1 with the terpene tackifying resin and the curing agent, stirring evenly, then scraping the film on the release film, and heating and drying at 120±5° C. for 0.5-5 min to obtain a skin low-sensitivity pressure-sensitive adhesive.

[0015] Preferably, the polyacrylic resin is composed of methyl acrylate, butyl acrylate, methyl methacrylate, hydroxyethyl methacrylate and an initiator in a mass ratio of 5:10:4:1.

[0016] Beneficial effect: Compared with the prior art, the present invention reduces the content of impurities in the resin by: first, selecting monomers with higher purity, wherein the purity is 98-100%; second, controlling the monomer conversion rate to be above 99% during the preparation process; third, controlling the VOC of the tape, wherein the VOC is 0-500ppm; fourth, the selection of monomer types also has certain requirements, so as to reduce the content of impurities in the resin and reduce or avoid the use of irritating monomers, and at the same time, a certain amount (≥5%) of hydrophilic monomers must be contained to reduce skin sensitivity. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms of the present invention by those skilled in the art all fall within the scope defined by the appended claims of the present application.

[0018] The skin-sensitive pressure-sensitive adhesive resin composition of the present invention includes an acrylic pressure-sensitive adhesive resin, a tackifying resin, a curing agent, etc. The following introduces the pressure-sensitive adhesive tape made of the pressure-sensitive adhesive resin composition of the present invention and its preparation method through examples and comparative examples. Example

[0019] Weigh 25g of methyl acrylate, 50g of butyl acrylate, 20g of methyl methacrylate, and 5g of 2-hydroxyethyl methacrylate, mix them evenly with 1% of AIBN, and set aside. Weigh 100g of ethyl acetate, put it into the bottom of the reactor and stir evenly, and fill it with nitrogen to deoxygenate for one hour. Raise the system temperature to 70°C, drip the mixed solution of monomer and initiator into the reactor within three hours, and keep it warm for 4 hours to obtain resin A. The viscosity of resin A is 5650mPa·s, and its monomer conversion rate is tested.

[0020] Take 50g of resin A, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the VOC, 180° peel strength, holding force and residual adhesive of the tape.

[0021] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin. Example

[0022] Take 50g of resin A, add 10g of terpene tackifying resin and 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the VOC, 180° peel strength, holding force and residual adhesive of the tape.

[0023] Comparative Example 1:

[0024] The same amount of monomers as in Example 1 was used. 100 g of ethyl acetate was weighed and put into the bottom of the reaction kettle for uniform stirring. The mixture was deoxygenated for one hour by nitrogen filling. The system temperature was raised to 70°C. The mixed solution of monomers and initiators was dripped into the reaction kettle within three hours and kept warm for 2 hours. Resin B was obtained. The viscosity of the resin was 3765 mPa·s. The monomer conversion rate was tested.

[0025] Take 50g of resin B, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the tape is 150μm. Test the VOC, 180° peel strength, holding force and residual adhesive of the tape.

[0026] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin.

[0027] Comparative Example 2:

[0028] Take 50g of resin A, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 30s. The thickness of the prepared tape is 150μm. Test the VOC, 180° peel strength, holding force and residual adhesive of the tape.

[0029] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin.

[0030] Comparative Example 3

[0031] Weigh 18g of methyl methacrylate, 50g of butyl acrylate, 30g of isobornyl methacrylate, and 2g of 2-hydroxyethyl methacrylate, mix well with 1% AIBN, and set aside. Weigh 100g of ethyl acetate, put it into the bottom of the reactor and stir evenly, and fill it with nitrogen to deoxygenate for one hour. Raise the system temperature to 70°C, drip the mixed solution of monomer and initiator into the reactor within three hours, and keep it warm for 4 hours to obtain resin C. The viscosity of resin C is 3500 mPa·s, and its monomer conversion rate is tested.

[0032] Take 50g of resin C, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the VOC, 180° peel strength, holding force and residual adhesive of the tape.

[0033] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin.

[0034]

[0035] From the test results, it can be seen that when the monomer conversion rate of the resin does not reach 99%, more problems will occur in Comparative Example 1 compared with Example 1, such as decreased adhesion and slight residual adhesive after peeling. This is because the monomer has not reacted completely, and its molecular weight is lower than that of the resin that has reacted completely, and the cohesion is low. Cohesive failure occurs during peeling, resulting in residual adhesive. At the same time, the skin patch was peeled off after 4 hours and found to have slight redness. This is due to the irritation of the residual monomer to the skin. In addition, when the baking time is too short and the VOC of the tape is too high, there are residual solvents in the system, which can also easily lead to skin allergies and redness.

[0036] The inventors have rationally compounded soft and hard monomers and selected monomers with a lower glass transition temperature (Tg) (such as methyl acrylate, butyl acrylate, etc. in the embodiments) to mainly provide viscoelasticity, which mainly provides initial adhesion; at the same time, the hard monomers of methyl methacrylate or ethyl methacrylate are combined to have a higher Tg, which improves the resin modulus and cohesion. More importantly, when synthesizing polyacrylic resins, the present invention selects hydrophilic monomers so that the prepared pressure-sensitive adhesive has better air permeability and water permeability, and reduces the skin sensitivity of the pressure-sensitive adhesive. For example, compared with Example 1, Comparative Example 3 has a lower content of hydrophilic monomers, and after being attached to the skin, sweat cannot be discharged due to infiltration, resulting in wrinkles after long-term attachment.

[0037] Compared with conventional pressure-sensitive adhesives, the present invention improves and controls the reaction conversion rate to more than 99%, with the aim of reducing the residual small molecule components of the product, thereby further reducing the skin sensitivity of the pressure-sensitive adhesive.

[0038] At the same time, through the selection of monomers, hydrophilic monomers must be contained, and the content must be ≥5%. The purpose is to reduce the long-term accumulation of sweat between the tape and the skin and irritation to the skin, so as to further reduce the skin sensitivity of the pressure-sensitive adhesive. Example

[0039] Weigh 25g of ethyl acrylate, 30g of butyl acrylate, 20g of isooctyl acrylate, 15g of methyl methacrylate, 5g of 2-hydroxyethyl methacrylate, 5g of N-vinyl pyrrolidone and 1% of AIBN and mix them evenly for use. Weigh 100g of ethyl acetate and put it into the bottom of the reactor and stir evenly. Fill with nitrogen to deoxygenate for one hour. Raise the system temperature to 70℃, drip the mixture of monomer and initiator into the reactor within three hours, and keep it warm for 4 hours. Resin C is obtained, the viscosity of which is 6000 mPa·s, and its monomer conversion rate is tested.

[0040] Take 50g of resin C, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the 180° peeling force, holding force and residual adhesive of the tape.

[0041] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin. Example

[0042] Weigh 14g ethyl acrylate, 55g butyl acrylate, 15g methyl methacrylate, 5g 2-hydroxyethyl methacrylate, 3g N-vinyl pyrrolidone, 8g vinyl acetate and 1% AIBN and mix them evenly for use. Weigh 100g ethyl acetate and put it into the bottom of the reactor and stir evenly. Fill with nitrogen to deoxygenate for one hour. Raise the system temperature to 70℃, drip the mixture of monomer and initiator into the reactor within three hours, and keep it warm for 4 hours. Resin D is obtained, the viscosity of which is 4000 mPa·s, and its monomer conversion rate is tested.

[0043] Take 50g of resin D, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the 180° peeling force, holding force and residual adhesive of the tape.

[0044] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin. Example

[0045] Weigh 75g butyl acrylate, 17g methyl methacrylate, 5g 2-hydroxyethyl methacrylate, 3g N-vinyl pyrrolidone and 1% AIBN and mix them evenly for standby use. Weigh 100g ethyl acetate and put it into the bottom of the reactor and stir evenly. Fill with nitrogen to deoxygenate for one hour. Raise the system temperature to 70℃, drip the mixture of monomer and initiator into the reactor within three hours, and keep it warm for 4 hours. Resin E is obtained, the viscosity of which is 3200 mPa·s, and its monomer conversion rate is tested.

[0046] Take 50g of resin E, add 0.1g of curing agent N3390, stir evenly, scrape the film on the release film, and dry it in an oven at 120℃ for 5min. The thickness of the prepared tape is 150μm. Test the 180° peeling force, holding force and residual adhesive of the tape.

[0047] Apply the tape to the skin of your arm, peel it off after 4 hours, and check the condition of your skin.

[0048]

[0049] The test results show that when the soft monomer content is high, the 180° peeling force is higher, but the holding force will decrease, and even residual adhesive will appear after peeling. If irritating substances such as vinyl acetate are added to the resin, after the pressure-sensitive adhesive is applied to the skin for 4 hours, slight redness will be found after peeling.

[0050] This method can be applied to all methods of reducing skin sensitivity by controlling the conversion rate of monomers, selecting monomer types, and controlling the VOC of pressure-sensitive adhesives, and is not limited to the types proposed in the examples. With the development of the medical field, higher requirements may be put forward for skin contact time. This method is not only limited to the 4-hour attachment in the examples, but also applicable to skin attachment for a longer period of time. At the same time, the resin prepared by this method has good transparency and can also be used for pressure-sensitive adhesives in other applications with transparency requirements.

[0051] The low skin sensitivity pressure-sensitive adhesive resin provided by the present invention uses raw materials with a purity of more than 98%. Compared with the prior art, which has no special requirements for the conversion rate (usually more than 92%), the present invention controls the monomer conversion rate to more than 99% during the reaction preparation process, on the one hand to reduce the residual small molecule monomers, and on the other hand to control the VOC content in the finished tape to less than 500ppm, thereby reducing the skin sensitivity of the pressure-sensitive adhesive. In addition, the present invention uses hydrophilic monomers, such as methyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, etc., to improve the air permeability of the pressure-sensitive adhesive, thereby improving the discomfort to human skin when the skin is applied.

[0052] The above descriptions are only some embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A pressure-sensitive adhesive resin composition with low skin sensitivity, characterized in that: The pressure-sensitive adhesive resin composition is composed of 50-98wt% polyacrylic acid resin, 0-50wt% tackifying resin and 0.01-2wt% curing agent. The VOC content of the pressure-sensitive adhesive resin composition is controlled below 500ppm, and the conversion rate of each monomer exceeds 99%. The polyacrylic acid resin is obtained by reacting methyl acrylate, butyl acrylate, methyl methacrylate, hydroxyethyl methacrylate and an initiator in a mass ratio of 5:10:4:

1.

2. The pressure-sensitive adhesive resin composition with low skin sensitivity according to claim 1, characterized in that: The purity of the raw materials of the pressure-sensitive adhesive resin composition is above 98%, and the content of carcinogens and allergens in the raw materials accounts for less than 0.1% of the total weight of the pressure-sensitive adhesive resin composition.

3. The pressure-sensitive adhesive resin composition with low skin sensitivity according to claim 2, characterized in that: The initiator is azobisisobutyronitrile or benzoyl peroxide; the tackifying resin is rosin resin or terpene resin; and the model of the curing agent is N3390.

4. A method for preparing a pressure-sensitive adhesive tape based on the pressure-sensitive adhesive resin composition with low skin sensitivity according to any one of claims 1 to 3, characterized in that The following steps are involved: S1, preparation of polyacrylic acid resin: soft monomer, hard monomer, functional monomer and initiator are uniformly mixed according to mass ratio to obtain a mixture of monomer and initiator; a proper amount of solvent ethyl acetate is added into a reaction kettle, and nitrogen is flushed in to deoxygenate for at least 1 hour, the system is heated to 70±3° C., and the mixture of monomer and initiator is slowly dripped into the reaction kettle within 2-5 hours, and the mixture is kept warm for polymerization reaction for 3-5 hours, and the reaction is stopped when the monomer conversion rate reaches more than 99% to obtain a polyacrylic acid resin with a viscosity of 3000-7000 mPa·s; S2, mixing the polyacrylic acid resin obtained in step S1 with a tackifying resin and a curing agent, stirring evenly, then scraping a film on a release film, and heating and drying at 120±5° C. for 0.5-5 min to obtain a skin low-sensitivity pressure-sensitive adhesive.

Citation Information

Patent Citations

  • Environment-friendly medical polyacrylate pressure-sensitive adhesive

    CN105219317A

  • Medical pressure-sensitive adhesive composition, preparation method thereof and adhesive material

    CN111876102A

  • Process for preparing solvent-type acrylic pressure-sensitive adhesives and medical pressure-sensitive adhesive

    CN1179782A

  • Adhesive pressure tape

    KR1020050051090A

  • KR20200016092A