A steam-free active admixture concrete material for concrete poles and preparation method thereof

Through the use of steam-curing-free active admixtures and active activators, the problems of high resource consumption and low preparation efficiency of high-temperature steam curing of traditional concrete poles are solved, and concrete pole materials with excellent mechanical properties can be efficiently prepared at room temperature, reducing the project costs and environmental impact.

CN118307227BActive Publication Date: 2024-10-01NORTHEAST DIANLI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410409529.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-01
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

Traditional concrete poles consume a lot of resources during high-temperature steam-curing, have low preparation efficiency, and require special equipment and construction conditions, which limits the feasibility of the project.

Method used

Use steam-free active admixtures, including blast furnace slag, microbead fly ash, silica fume, metakaolin, quicklime and corn straw fermentation, combined with active activators such as silica sol, potassium hydroxide and vinyl n-butyrate/modified The natural lignin compound, through a specific mixing and fermentation process, forms a highly efficient concrete material.

Benefits of technology

It significantly improves the early strength and durability of concrete at room temperature, reduces preparation costs and resource consumption, avoids the need for high-temperature steam curing, and improves construction efficiency and sustainability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004778662640000081
    Figure BDA0004778662640000081
  • Figure BDA0004778662640000082
    Figure BDA0004778662640000082
  • Figure BDA0004778662640000091
    Figure BDA0004778662640000091
Patent Text Reader

Abstract

The invention discloses a non-steaming active admixture concrete material for concrete poles and a preparation method thereof, and belongs to the technical field of concrete preparation. The non-steaming active admixture concrete material for concrete poles of the invention comprises raw materials including: 10 parts by mass of non-steaming active admixture, 10 parts by mass of cement, 30 parts by mass of fine aggregate, 40 parts by mass of coarse aggregate, 10 parts by mass of water and an active stimulant; the non-steaming active admixture comprises blast furnace slag, micro-bead fly ash, silica fume, metakaolin, quicklime and corn stalk fermentation. The non-steaming active admixture concrete material for concrete poles of the invention can obtain good mechanical properties, working performance and corrosion resistance without using a steaming method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete preparation, in particular to a steam-curing-free active admixture concrete material for concrete poles and a preparation method thereof. Background Art

[0002] Concrete poles are widely used as supporting structures for power transmission and telecommunication lines, and their performance is related to the reliability and safety of power and communication systems. Although traditional pole materials, such as wood and steel, meet the structural requirements of poles to a certain extent, they are also accompanied by a series of problems, such as decay, corrosion, and excessive weight, which may lead to a shortened life of poles, increased maintenance costs, and increased environmental impact. In order to improve the strength, stability, and durability of poles, concrete poles have become a popular choice. However, the use of concrete materials in concrete poles is crucial because it directly affects the mechanical properties and durability of the poles. In traditional concrete poles, high-temperature steam curing is usually required to improve the early strength of concrete, but the current steam curing technology requires too many preparation resources and the preparation efficiency is usually low. In addition, high-temperature steam curing usually requires special equipment and construction conditions, which will be limited in some engineering projects. Summary of the invention

[0003] The purpose of the present invention is to provide a steam-curing-free active admixture concrete material for concrete poles and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] One of the technical solutions of the present invention is a steam-free active admixture, which comprises the following raw materials in parts by weight: 20-40 parts of blast furnace slag, 20-30 parts of micro-bead fly ash, 25-40 parts of silica fume, 5 parts of metakaolin and 5 parts of quicklime.

[0006] Furthermore, the steam-free active admixture further comprises 20 to 25 portions of corn stalk fermentation material.

[0007] Furthermore, the method for preparing the corn stalk fermentation product comprises the following steps:

[0008] The corn stalks are crushed, added to a mixed solution of urea, calcium persulfate and gypsum powder, stirred evenly, and then a fermentation agent is added, mixed evenly, and then piled for fermentation to obtain fermented stalks;

[0009] The fermented corn stalks are dried and then crushed to obtain the corn stalk fermentation product.

[0010] Furthermore, the mass ratio of the corn stalks, urea, calcium persulfate and gypsum powder is 100:1:0.2:0.2;

[0011] The fermentation agent comprises the following components in parts by weight: 2-3 parts of yeast, 1-2 parts of lactic acid bacteria, 4-5 parts of green mold, 1-2 parts of black mold and 2-3 parts of white rot fungi;

[0012] The temperature of the pile fermentation is 45-50°C and the time is 45-50 days.

[0013] The second technical solution of the present invention: A steam-free active admixture concrete material for concrete poles, the raw materials including: 10 parts by mass of the above-mentioned steam-free active admixture, 10 parts by mass of cement, 30 parts by mass of fine aggregate, 40 parts by mass of coarse aggregate, 10 parts by mass of water and an activity activator.

[0014] Furthermore, the active activator includes gypsum, silica sol and potassium hydroxide; the mass ratio of the gypsum, silica sol and potassium hydroxide is 1:(1-1.5):(0.8-1); the total amount of the gypsum, silica sol and potassium hydroxide is 1.8-3.5% of the mass of cement.

[0015] Furthermore, the activity stimulator also includes a composite of vinyl butyrate / modified lignin; the amount of the composite of vinyl butyrate / modified lignin is 3-5% of the mass of cement.

[0016] Furthermore, the method for preparing the vinyl butyrate / modified lignin composite comprises the following steps:

[0017] Add lignin to water, mix well, add sodium hydroxide to adjust the pH to alkaline, then heat and stir to react, and drop formaldehyde solution during the heating and stirring reaction, and obtain modified lignin after the reaction is completed;

[0018] Vinyl n-butyrate, modified lignin and an initiator are mixed, heated and refluxed to react, so as to obtain the vinyl n-butyrate / modified lignin composite.

[0019] The third technical solution of the present invention is a method for preparing the above-mentioned steam-curing-free active admixture concrete material for concrete poles, comprising the following steps:

[0020] The active stimulant and water are mixed and stirred to obtain a mixture 1 (active stimulant solution);

[0021] After fine aggregate and coarse aggregate are dry-mixed evenly, cement and autoclaved active admixture are added and stirred evenly to obtain mixture 2;

[0022] The mixture 1 is added into the mixture 2 and stirred evenly to obtain the steam-curing-free active admixture concrete material for the concrete pole.

[0023] A fourth technical solution of the present invention: an application of the above-mentioned steam-curing-free active admixture concrete material in the preparation of concrete poles.

[0024] Blast furnace slag is a byproduct of the ironmaking process and is usually the residue from the smelting of iron ore in a blast furnace. Blast furnace slag contains components such as silicon, aluminum and calcium, which can play an active role in the cement hydration reaction. Adding an appropriate amount of blast furnace slag can improve the early and long-term strength of concrete, while improving its durability and making concrete more resistant to environmental erosion.

[0025] Fly ash hollow microspheres (hollow microspheres for short) are spherical fly ash collected from the chimney emissions of coal-fired thermal power plants by professional equipment. They have the characteristics of small particle size and high activity. Introducing hollow microspheres into concrete can help reduce the viscosity of concrete, reduce water consumption, and improve the pore structure, thereby increasing the strength of concrete, and can improve the fluidity and plasticity of concrete, and improve the working performance of concrete.

[0026] Silica fume is a fine powder mineral admixture that can fill the pores in concrete, improve the density, strength, durability and crack resistance of concrete, reduce permeability, and reduce the risk of thermal cracks. In addition, silica fume can also help reduce the amount of cement in concrete, thereby reducing carbon emissions and costs, in line with the principles of sustainable construction. In short, the addition of silica fume makes concrete stronger and more durable, helping to improve its performance and sustainability.

[0027] Metakaolin is a natural mineral that can be added to concrete as a mineral admixture to help increase the fluidity of concrete, improve workability, and make concrete easier to pour and process. In addition, metakaolin can increase the viscosity of concrete and help reduce the tendency of concrete to crack.

[0028] The main component of quicklime is calcium oxide (CaO). Its application in concrete has multiple effects, including promoting hardening reaction, improving working performance (filling pores and increasing fluidity), adjusting setting time, improving impermeability and durability, etc. Quicklime can adapt to different construction needs and provide more reliable building materials for projects.

[0029] The steam-free active admixture of the present invention is more active than a single material. By adding it to concrete, concrete with better mechanical properties can be prepared and the cost can be reduced. Compared with single active admixtures, reasonable mixing can significantly improve the microscopic morphology, hydration products, and pore structure of concrete, and can well coordinate its influence on the workability of concrete mixtures, and improve the strength more significantly. Each admixture cooperates with each other, giving full play to the "composite super-superposition effect", and the particle gradation is optimized to the maximum, thereby improving the mechanical properties of concrete.

[0030] In a preferred embodiment of the present invention, the steam-free active admixture concrete material for concrete poles contains corn straw fermentation products, and the active stimulant contains vinyl butyrate / modified lignin; the corn straw fermentation products contain a variety of active groups, such as carboxyl, phenolic hydroxyl, alcohol hydroxyl, ketone, amide, etc., which can react with the complex of vinyl butyrate / modified lignin to form larger molecular chains that are filled in the concrete system, further provide reinforcement, and enhance the early strength of the concrete.

[0031] The active activator of the present invention contains silica sol, which can accelerate the hydration reaction of cement and provide silicon dioxide required for the hydration reaction, thereby improving the early strength of concrete. Silica sol also helps to reduce the risk of thermal cracking of concrete and improve crack resistance. In addition, the microscopic particle structure of silica sol can fill the micropores in concrete, improve the density and durability of concrete, and silica sol can also reduce the permeability of concrete, thereby improving its ability to resist chemical erosion, chloride erosion and sulfate erosion.

[0032] The activity activator of the present invention contains potassium hydroxide. After potassium hydroxide is added, an alkaline environment can be provided for concrete. Under alkaline conditions, the active admixture is easy to form ettringite, and the dissolution of the active admixture can be accelerated and the hydration rate of C2S and C3S can be increased. In addition, potassium ions can depolymerize the glass by changing the network structure of the silicate glass, thereby activating the activity of the active admixture.

[0033] The active activator of the present invention contains raw gypsum, which can provide sulfate ions to promote the formation of ettringite, and because the active admixture lacks a lot of Ca compared with cement, 2+ , Ca provided only by calcium hydroxide produced by cement hydration 2+ It is not enough to meet the demand, so the calcium ions in gypsum can appropriately supplement the hydration system.

[0034] The active stimulant of the present invention contains a composite of vinyl butyrate / modified lignin, which contains multiple polar groups such as ester groups, carboxyl groups, hydroxyl groups, etc., and can improve the compatibility between concrete raw materials, thereby improving the early strength of concrete. At the same time, the acidic groups in the composite of vinyl butyrate / modified lignin can work together with potassium hydroxide to promote the growth of calcium carbonate crystals, form a self-compacting concrete bonding interface, block the capillary channels inside the concrete, greatly improve the performance of the concrete system in resisting chloride ion penetration, and can provide a certain elasticity in the concrete during the application process, ensure the stability of the concrete system, and improve the early strength and the effect of resisting chloride ion penetration from another aspect.

[0035] The mixed active stimulant (active stimulant) of the present invention has a better stimulating effect than a single stimulant, and can significantly improve the early strength of concrete. The mixed active stimulant of the present invention can not only promote the hydration reaction of cement, but also stimulate the early activity of active admixtures, accelerate the cracking and hydration of active admixtures under the joint action of potassium-calcium-sulfur, and at the same time provide the necessary calcium ions for forming cementitious materials, which can quickly improve the early strength.

[0036] The present invention discloses the following technical effects:

[0037] (1) The steam-free active admixtures of the present invention are all admixtures that can fully exert their activity in concrete, are less affected by chloride ion or sulfate ion corrosion, have stronger durability, and can further reduce the human resources and costs required for later maintenance. A reasonable mixing method of the steam-free active admixtures can fully exert their synergistic effect in concrete, improve the microstructure of concrete and enhance the degree of hydration reaction.

[0038] (2) The active activator of the present invention can effectively improve the performance of concrete and enhance the early strength of concrete.

[0039] (3) The steam-curing-free active admixture concrete material for concrete poles of the present invention can obtain good mechanical properties, working performance and corrosion resistance without using a steam-curing method.

[0040] (4) The steam-curing-free active admixture concrete material for concrete poles of the present invention does not require the use of high-temperature equipment for steam curing and high-pressure curing, which can reduce the preparation cost of concrete, save a lot of manpower and material resources, reduce engineering costs, and improve the efficiency and sustainability of concrete construction, reduce resource waste, reduce energy consumption, improve the performance of concrete, and help alleviate environmental pressure.

[0041] (5) The compressive strength of the steam-free active admixture concrete material for concrete poles of the present invention is greatly improved compared with ordinary concrete. It can harden at room temperature and reach the required strength without the need for additional wet curing or steam curing process. It has a good early strength effect and can avoid the problem of poor later durability due to the increase in early strength. DETAILED DESCRIPTION

[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0043] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0047] The “parts” described in the following examples are all “parts by mass”.

[0048] The raw materials used in the present invention are as follows:

[0049] (1) The particle size of blast furnace slag is 20-30 μm, and the chemical composition is as follows:

[0050] Table 1 Chemical composition of blast furnace slag (wt.%)

[0051] Element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO CaO <![CDATA[SO3]]> Impurities content 31.26 15.56 1.14 8.75 36.14 0.21 6.94

[0052] (2) The particle size of fly ash hollow microspheres is 0.5-1 μm, and the chemical composition is as follows:

[0053] Table 2 Chemical composition of fly ash hollow microspheres (wt.%)

[0054] Element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO CaO <![CDATA[K2O]]> Impurities content 60.15 32.21 3.05 0.86 0.77 0.25 2.71

[0055] (3) The average particle size of silica fume is 0.18 μm.

[0056] (4) The particle size of metakaolin is 2 to 4 μm.

[0057] (5) The particle size of quicklime is 35 to 70 μm.

[0058] (6) The cement is silicate cement P·O 42.5.

[0059] (7) The fine aggregate is sand with a particle size of 1 to 3.2 mm.

[0060] (8) The coarse aggregate is crushed stone with a particle size between 10 and 15 mm.

[0061] (9) Silica sol is neutral silica sol purchased from Guangzhou Zhonggao Chemical Co., Ltd.

[0062] (10) The yeast, lactic acid bacteria, Trichoderma viride, Aspergillus niger and white rot fungi used in the present invention are all commercially available, and the number of effective live bacteria is 500 million to 1 billion per gram.

[0063] Example 1

[0064] A method for preparing a steam-free active admixture concrete material for concrete poles:

[0065] The components in Table 3 and Table 4 were used as raw materials to prepare the steam-free active admixture concrete materials, as follows:

[0066] Table 3 Concrete with different mass proportions

[0067]

[0068] The mass proportions of the steam-free active admixtures corresponding to the concretes of each serial number are shown in Table 4.

[0069] Table 4 Mass proportion of steam-free active admixtures

[0070]

[0071]

[0072] Serial numbers 0 to 9 represent 10 different types of concrete.

[0073] Preparation method of concrete No. 1 to 8:

[0074] (1) After mechanical ball milling, blast furnace slag and hollow microspheres are mixed with silica fume, metakaolin and quicklime powder, and stirred evenly to obtain a steam-free active admixture.

[0075] (2) Gypsum, silica sol, potassium hydroxide and water are mixed and stirred thoroughly to obtain an active activating solution.

[0076] (3) Pour the fine aggregate and coarse aggregate into a mixer and dry mix for 1 min. Then add cement and steam-free active admixture and continue mixing for 2 min to obtain mixture 1.

[0077] (4) Add the active stimulating solution into mixture 1 and stir thoroughly for 1 min to obtain mixture 2.

[0078] (5) Mixture 2 is placed in a mold and vibrated to form, and then demolded after being placed in a room temperature environment (ambient temperature is 20±2° C., humidity is 50-60%) for 24 hours to obtain a steam-free active admixture concrete material for concrete poles.

[0079] Preparation method of concrete No. 0:

[0080] (1) Cement, fine aggregate, coarse aggregate and water are mixed and stirred uniformly to obtain a mixture.

[0081] (2) The mixture is placed in a mold and vibrated to form, and then placed in a room temperature environment (ambient temperature is 20±2° C., humidity is 50-60%) for 24 hours before demolding to obtain a concrete material.

[0082] Preparation method of concrete No. 9:

[0083] (1) After mechanical ball milling, blast furnace slag and hollow microspheres are mixed with silica fume, metakaolin and quicklime powder, and stirred evenly to obtain a steam-free active admixture.

[0084] (2) Pour the fine aggregate and coarse aggregate into a mixer and dry mix for 1 min. Then add cement, steam-free active admixture and water and continue mixing for 2 min to obtain mixture 1.

[0085] (3) Mixture 1 is placed in a mold and vibrated to form, and then placed in a room temperature environment (ambient temperature is 20±2° C., humidity is 50-60%) for 24 hours and then demolded to obtain a concrete material.

[0086] According to the test method described in GB / T50081-2019 "Test Method for Mechanical Properties of Ordinary Concrete" (traditional steam curing was not performed, and the concrete material obtained after demolding was placed in a standard concrete curing box for curing), the compressive strength of concrete materials No. 0 to 9 prepared in this embodiment was measured, and the results are shown in Table 5.

[0087] Table 5 Compressive strength test results

[0088]

[0089] It can be seen from Tables 3 to 5 that the adjustment of the dosage of the steam-free active admixture components will affect the strength of the concrete, which further illustrates the synergistic effect of mineral admixtures. Only a reasonable mixing method can make the synergistic effect more fully exerted and promote the process of hydration reaction, thereby achieving the technical effect of improving the mechanical properties of concrete.

[0090] It can be seen from the concretes No. 1 to 8 that with the increase in the amount of silica sol added, the strength of the concrete at each stage gradually increases, indicating that silica sol can effectively improve the compressive strength of concrete.

[0091] From the concrete compressive strength test results of No. 4 and No. 8, it can be seen that when the slag content is increased and the hollow microspheres and silica fume content is reduced, the compressive strength of the concrete decreases slightly. This is because the slag content is too large and its own particle size is large, which changes the particle gradation of the concrete, resulting in more pores; and there are too many powder particles with large specific surface area, which hinders the hydration reaction rate. Hollow microspheres and silica fume have small particle sizes, and they can fill the pores when mixed into concrete, participate in the hydration reaction to generate hydration products, and make the matrix denser. Therefore, reducing the content of hollow microspheres and silica fume also leads to a decrease in the mechanical properties of concrete.

[0092] It can be seen from the concrete of No. 9 that due to the lack of active activator, the hydration reaction rate of the cementitious material is reduced, and the compressive strength of the obtained concrete is lower than that of other groups.

[0093] Example 2

[0094] The same as No. 6 of Example 1, except that the steam-free active admixture further contains 20 parts of corn stalk fermentation material.

[0095] Preparation method of corn straw fermentation product:

[0096] The corn stalks are crushed and added with a mixed aqueous solution of urea, calcium persulfate and gypsum powder (the mass ratio of corn stalks, urea, calcium persulfate and gypsum powder is 100:1:0.2:0.2), stirred evenly, and then a fermentation agent is added (the amount of the fermentation agent is 0.1% of the mass of the corn stalks), mixed evenly, and the water content is adjusted to about 50%, and the mixture is piled for fermentation (the temperature is 45°C and the time is 50 days). The pile is turned over every 10 days during the fermentation to obtain fermented straw.

[0097] The fermented corn straw is dried and crushed into 100 meshes to obtain corn straw fermentation product.

[0098] The starter consists of the following components in parts by weight: 3 parts of yeast, 2 parts of lactic acid bacteria, 4 parts of green Trichoderma, 1 part of black Aspergillus and 2 parts of white rot fungi.

[0099] Example 3

[0100] The same as No. 6 in Example 1, except that the raw material also contains a composite of vinyl butyrate / modified lignin, and the amount used is 4% of the mass of cement.

[0101] Preparation method of vinyl butyrate / modified lignin composite:

[0102] A. Add lignin to water (the mass / volume ratio of lignin to water is 1g:15mL), mix well, add sodium hydroxide to adjust the pH to 11, then heat and stir to react (temperature is 80°C, speed is 100r / min, time is 3h), and during the heating and stirring reaction, add dropwise a 35wt.% formaldehyde solution (the mass / volume ratio of lignin to formaldehyde solution is 1g:1mL). After the reaction is completed, dry and crush to 100 mesh to obtain modified lignin.

[0103] B. Vinyl butyrate, modified lignin and azobisisobutyronitrile were mixed in a mass ratio of 10:1.5:0.08, heated to reflux reaction (temperature of 80°C, time of 5h), and after the reaction, the solvent was removed, and the mixture was washed with deionized water and dried to obtain a vinyl butyrate / modified lignin complex.

[0104] Example 4

[0105] The same as No. 6 in Example 1, except that the steam-free active admixture further contains 20 parts of corn stalk fermentation material (preparation method is the same as Example 2).

[0106] The active activator also contains a composite of vinyl n-butyrate / modified lignin, the amount of which is 4% of the mass of cement (the preparation method is the same as that of Example 3).

[0107] Comparative Example 1

[0108] The same as sequence number 6 of Example 1, except that the amount of raw gypsum is 1% of the mass of cement, the amount of silica sol is 1.5% of the mass of cement, and the amount of potassium hydroxide is 5% of the mass of cement.

[0109] Comparative Example 2

[0110] The same as sequence number 6 of Example 1, the only difference is that the active activator is a composite of raw gypsum, silica sol and vinyl butyrate / modified lignin, the amount of raw gypsum is 1% by mass of cement, the amount of silica sol is 1.5% by mass of cement, and the amount of vinyl butyrate / modified lignin composite is 4% by mass of cement.

[0111] Comparative Example 3

[0112] The same as No. 6 of Example 1, except that the steam-free active admixture does not contain hollow microspheres and silica fume.

[0113] Comparative Example 4

[0114] The same as sequence number 6 of Example 1, except that the active activator is potassium hydroxide, and the amount used is 3.5% of the mass of cement.

[0115] According to the test method described in GB / T50081-2019 "Test Method for Mechanical Properties of Ordinary Concrete" (traditional steam curing was not performed, and the concrete material obtained after demolding was placed in a standard concrete curing box for curing), the compressive strength of the concrete materials prepared in Examples 2 to 4 and Comparative Examples 1 to 4 was measured, and the results are shown in Table 6.

[0116] Table 6 Compressive strength test results

[0117]

[0118] The reason for the decrease in strength of Comparative Example 1 is that the amount of potassium hydroxide, an active stimulant, is too large, while the composite of vinyl butyrate / modified lignin is not only used as an active stimulant, but also can improve the compatibility between concrete raw materials, thereby improving the early strength of concrete. Therefore, even when the amount used is significantly higher than that of other active stimulants, it will not lead to a decrease in the strength of the concrete, but will improve the strength of the concrete.

[0119] It can be seen from Table 6 that adding the corn straw fermentation product and the composite of vinyl butyrate / modified lignin prepared in the present invention to concrete can significantly improve the compressive strength of the concrete.

[0120] Effect Example 1

[0121] According to the standard NT BUILD 492, the chloride ion diffusion coefficient of concrete cured at room temperature for 28 days was determined. The results are shown in Table 7.

[0122] Table 7 Chloride ion diffusion coefficient of concrete

[0123]

[0124] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A non-steamed active admixture concrete material for concrete poles, characterized in that: The raw materials include: 10 parts by mass of steam-free active admixture, 10 parts by mass of cement, 30 parts by mass of fine aggregate, 40 parts by mass of coarse aggregate, 10 parts by mass of water and an active activator; The active activator comprises raw gypsum, silica sol, potassium hydroxide and a composite of vinyl butyrate / modified lignin; the mass ratio of the raw gypsum, silica sol and potassium hydroxide is 1:(1-1.5):(0.8-1); the total amount of the raw gypsum, silica sol and potassium hydroxide is 1.8-3.5% of the mass of cement; the amount of the composite of vinyl butyrate / modified lignin is 3-5% of the mass of cement; The method for preparing the vinyl butyrate / modified lignin composite comprises the following steps: adding lignin to water, mixing evenly, adding sodium hydroxide to adjust the pH to alkaline, then heating and stirring to react, and dropwise adding formaldehyde solution during the heating and stirring reaction, and obtaining modified lignin after the reaction is completed; Mixing vinyl butyrate, modified lignin and an initiator, and heating to reflux for reaction to obtain the vinyl butyrate / modified lignin composite; The steam-free active admixture comprises the following raw materials in parts by weight: 20 to 40 parts of blast furnace slag, 20 to 30 parts of micro-bead fly ash, 25 to 40 parts of silica fume, 5 parts of metakaolin, 5 parts of quicklime and 20 to 25 parts of corn stalk fermentation; The method for preparing the corn stalk fermentation product comprises the following steps: The corn stalks are crushed, added into a mixed solution of urea, calcium persulfate and gypsum powder, stirred evenly, and then a fermentation agent is added, mixed evenly and then piled for fermentation to obtain fermented stalks; drying and crushing the fermented corn stalks to obtain the corn stalk fermentation product; The mass ratio of the corn stalks, urea, calcium persulfate and gypsum powder is 100:1:0.2:0.2; The fermentation agent comprises the following components in parts by weight: 2-3 parts of yeast, 1-2 parts of lactic acid bacteria, 4-5 parts of green mold, 1-2 parts of black mold and 2-3 parts of white rot fungi; The temperature of the pile fermentation is 45-50°C and the time is 45-50 days.

2. A method for preparing the autoclaved-free active admixture concrete material for concrete poles according to claim 1, characterized in that: The following steps are involved: The active stimulant and water are mixed and stirred to obtain a mixture 1; After fine aggregate and coarse aggregate are dry-mixed evenly, cement and autoclaved active admixture are added and stirred evenly to obtain mixture 2; The mixture 1 is added into the mixture 2 and stirred evenly to obtain the steam-curing-free active admixture concrete material for the concrete pole.

3. Use of the autoclaved-free active admixture concrete material according to claim 1 in the preparation of concrete poles.