Anchoring and elasticity reducing agent for shotcrete and preparation method thereof

By using anchoring elasticity reducing agents prepared from materials such as cross-linked bodies in shotcrete construction, the problem of high rebound rate of shotcrete is solved, achieving a high thickening effect with low dosage, reducing the rebound rate and improving the strength of concrete. Bond strength.

CN118307236BActive Publication Date: 2024-10-29GUANGDONG WUYUAN BUILDING MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410579851.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-10-29
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

The rebound rate in existing shotcrete construction is high, resulting in waste of concrete. The traditional method is costly, inefficient and difficult to control, and affects the later working strength of the concrete.

Method used

An anchor elasticity-reducing agent for shotcrete is used, including a thickener, a water-retaining agent, an air-entraining agent and a reinforcing agent. It is prepared through the graft copolymerization of cross-linked bodies, polyether monomers and small molecule monomers to form polymers. Aqueous solution thickener, improves the rheological properties and viscosity of concrete and reduces the rebound rate.

Benefits of technology

It effectively reduces the rebound rate of shotcrete from 20%-30% to less than 5%, improves the bonding strength and cohesion effect of concrete, avoids affecting the later work intensity, and reduces the dosage and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307236B_ABST
    Figure CN118307236B_ABST
Patent Text Reader

Abstract

The present application discloses an anchoring and elasticity reducing agent for shotcrete and a preparation method thereof, and relates to the technical field of concrete building materials. An anchoring and elasticity reducing agent for shotcrete, in terms of mass percentage, comprises the following raw materials: 40%-60% thickener, 0.02%-0.5% water retaining agent, 0.05%-0.5% air entraining agent, 5%-10% reinforcing agent and residual water; wherein the raw materials of the thickener include a cross-linked body, a polyether monomer, a small molecule monomer and an initiator. The anchoring and elasticity reducing agent of the present application can achieve the effect of low dosage and high thickening, can enhance the bonding and anchoring effect between the shotcrete and the base layer, avoid affecting the working strength of the shotcrete in the later stage, and can also enhance the cohesive effect between the concrete, thereby reducing the rebound rate of the shotcrete from 20%-30% to less than 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of concrete building materials, and in particular to an anchoring and elasticity reducing agent for shotcrete and a preparation method thereof. Background Art

[0002] Shotcrete is a construction method that uses a spraying machine to spray quick-setting concrete onto the surface of rocks or structures to strengthen and protect them. Shotcrete technology is mainly used for temporary support of tunnels and shaft excavations, and permanent or temporary support of excavated slopes. Nowadays, with the rapid development of infrastructure, the use of shotcrete has continued to grow, but in the process of shotcrete construction, due to the high rebound rate of shotcrete, a large amount of concrete will be wasted. According to statistics from a large number of projects, the rebound rate of shotcrete is between 20% and 30%. In order to reduce the rebound rate, most viscosity-enhancing composite materials are currently used to improve the cohesive properties of concrete, which mainly include mineral admixtures such as silica fume, fly ash, ultrafine limestone powder and ultrafine slag powder. The purpose of reducing the rebound rate is achieved by adjusting the concrete mix ratio, optimizing the wet spraying construction process, etc. However, the traditional method of adding ultrafine mineral admixtures to reduce the rebound rate of shotcrete has the disadvantages of high cost, low efficiency, and great control difficulty. The rebound rate is not effectively suppressed and the later working strength of the concrete is affected. Based on this, the present application proposes an anchoring and rebound reducing agent for shotcrete and a preparation method thereof. Summary of the invention

[0003] The main purpose of the present application is to provide an anchoring elasticity reducing agent for shotcrete and a preparation method thereof, aiming to solve the technical problem that the existing elasticity reducing agent has an unsatisfactory effect on reducing the rebound rate of shotcrete.

[0004] To achieve the above-mentioned purpose, the present application proposes an anchoring elasticity reducing agent for shotcrete, which comprises the following raw materials by mass percentage: 40%-60% thickener, 0.02%-0.5% water retaining agent, 0.05%-0.5% air entraining agent, 5%-10% reinforcing agent and the balance water;

[0005] The raw materials of the thickener include a cross-linker, a polyether monomer, a small molecule monomer and an initiator.

[0006] Optionally, the cross-linked body is a spatial network colloid comprising guar gum and xanthan gum, wherein the mass ratio of guar gum to xanthan gum is 3:2.

[0007] Optionally, the cross-linked body further comprises at least one of hydroxymethyl cellulose ether, hydroxyethyl cellulose ether and soluble starch ether.

[0008] Optionally, the polyether monomer includes one of isopentanol polyoxyethylene ether, 3-methylbut-3-enyl polyethylene glycol ether, 2-methylprop-2-enyl polyethylene glycol ether, ethylene glycol monovinyl polyoxyethylene ether and 4-hydroxybutyl vinyl polyoxyethylene ether.

[0009] Optionally, the small molecule monomers include at least two of acrylamide, acrylic acid, methacrylic acid, hydroxypropyl methacrylate and N,N-dimethylacrylamide.

[0010] Optionally, the preparation step of the thickener comprises:

[0011] After heating the water to 55-65°C, add guar gum and xanthan gum, stir for 0.8-1.2h until dissolved, add polyether monomer, small molecule monomer and initiator, stir for 3-8min, let stand for 1.5-2.5h, then add 55-65°C water, stir for 8-12min, swell for 1.5-2.5h, while keeping the temperature at 55-65°C. After swelling, stir at 40-50°C for 10-14h, then add lignin solution and sodium hydroxide, stir for 10-20min to obtain the finished thickener.

[0012] Optionally, the water retaining agent includes one of polyacrylamide and polyoxyethylene.

[0013] Optionally, the air entraining agent includes one of K12, AOS and AES.

[0014] Optionally, the enhancer includes one of calcium formate, sodium carbonate and sodium sulfate.

[0015] The present application also proposes a method for preparing an anchoring elasticity reducing agent for shotcrete, comprising the following steps:

[0016] Add water into the reaction kettle, then add the water retaining agent, after it dissolves, then add the reinforcing agent, thickener and air entraining agent in sequence, stir for 30min-60min, and obtain the finished anchoring elasticity reducing agent.

[0017] The anchoring elasticity reducing agent of the present application uses thickener, water-retaining agent, air-entraining agent and reinforcing agent as raw materials, and the thickener uses cross-linked body, polyether monomer, small molecule monomer and initiator as raw materials. The thickener of the present application is different from the molecular structure of single commercial thickeners such as xanthan gum, maltodextrin, cellulose ether, etc., and is also different from the simple physical mixture of two or more commercial thickeners. Instead, it is a product obtained by grafting copolymerization reaction with polyether monomer, small molecule monomer, etc. based on the spatial network structure of the cross-linked body. Compared with the dissolution process of thickeners such as cellulose ether and maltodextrin, which first swells and then dissolves, the feeding method and insufficient stirring time will lead to poor dissolution of this type of thickener, thereby affecting the homogeneity of the product. The thickener of the present application is a polymer aqueous solution, which has good water solubility and better stability in aqueous solution, is not easy to precipitate or precipitate, and has a good improvement effect on the rheological properties of concrete slurry, can increase the plastic viscosity of concrete slurry, and has a good bridging effect with concrete particles. Its mechanism of action includes water retention , association and bridging. The long-chain polymer molecules in the thickener are first adsorbed on the free water molecules, so that the mixing water in the concrete paste is fixed, so the plastic viscosity of the concrete increases. The long-chain polymer molecules will also be adsorbed on the surface of the concrete particles at the same time, thus forming a bridging structure of water-long-chain polymer molecules-concrete particles, forming a network of floccules, thereby enhancing the viscosity of the concrete and achieving a thickening effect; the water retaining agent also has a thickening function. The water retaining agent can effectively reduce the fluidity of the fresh concrete paste, making the concrete particles inside the fresh concrete paste easier to aggregate and form aggregates, further enhancing the effect of the thickener; the bubbles introduced by the air entraining agent play a lubricating role inside the paste to improve the wrapping of the concrete paste on the concrete aggregate, so that the produced concrete has better softness, and the soft paste can absorb the kinetic energy generated by the shotcrete during construction and reduce the rebound rate; the reinforcing agent is used to promote cement hydration and improve the bonding strength of the shotcrete. The anchoring elasticity reducing agent of the present application can achieve the effect of high thickening with low dosage, can enhance the bonding and anchoring effect between shotcrete and the base layer, avoid affecting the later working strength of shotcrete, and can also enhance the cohesion effect between concretes, thereby reducing the rebound rate of shotcrete from 20%-30% to less than 5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0019] Figure 1This is the infrared spectrum of the thickener described in the examples of this application.

[0020] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0022] In view of the technical problems existing in the prior art, the embodiment of the present application provides an anchoring elasticity reducing agent for shotcrete, which comprises the following raw materials by mass percentage: 40%-60% thickener, 0.02%-0.5% water retaining agent, 0.05%-0.5% air entraining agent, 5%-10% reinforcing agent and the balance water;

[0023] The raw materials of the thickener include a crosslinker, a polyether monomer, a small molecule monomer and an initiator. The thickener is a liquid product.

[0024] The anchoring elasticity reducing agent of the present application uses thickener, water retaining agent, air entraining agent and reinforcing agent as raw materials, and the thickener uses cross-linked body, polyether monomer, small molecule monomer and initiator as raw materials. The thickener of the present application is different from the molecular structure of single commercial thickeners such as xanthan gum, maltodextrin, cellulose ether, etc., and is also different from the simple physical mixture of two or more commercial thickeners. Instead, it is a product obtained by grafting copolymerization reaction with polyether monomer, small molecule monomer, etc. based on the spatial network structure of the cross-linked body. Compared with the dissolution process of thickeners such as cellulose ether and maltodextrin, which first swells and then dissolves, the feeding method and insufficient stirring time will lead to poor dissolution of this type of thickener, thereby affecting the homogeneity of the product. The thickener of the present application is a polymer aqueous solution, which has good water solubility and better stability in aqueous solution, is not easy to precipitate or precipitate, and has a good improvement effect on the rheological properties of concrete slurry, can increase the plastic viscosity of concrete slurry, and has a good bridging effect with concrete particles. Its mechanism of action includes retaining Water, association and bridging, the long-chain polymer molecules in the thickener are adsorbed on the free water molecules, so that the mixing water in the concrete paste is fixed, so the plastic viscosity of the concrete increases, and the long-chain polymer molecules are also adsorbed on the surface of the concrete particles, thereby forming a bridging structure of water-long-chain polymer molecules-concrete particles, forming a network of floccules, thereby enhancing the viscosity of the concrete and achieving a thickening effect; the water retaining agent also has a thickening function. The water retaining agent can effectively reduce the fluidity of the fresh concrete paste, making the concrete particles inside the fresh concrete paste easier to aggregate and form aggregates, further enhancing the effect of the thickener; the bubbles introduced by the air entraining agent play a lubricating role inside the paste to improve the wrapping of the concrete paste on the concrete aggregate, so that the produced concrete has better softness, and the soft paste can absorb the kinetic energy generated by the shotcrete during construction and reduce the rebound rate; the reinforcing agent is used to promote cement hydration and improve the bonding strength of the shotcrete. The anchoring elasticity reducing agent of the present application can achieve the effect of high thickening with low dosage, can enhance the bonding and anchoring effect between shotcrete and the base layer, avoid affecting the later working strength of shotcrete, and can also enhance the cohesion effect between concretes, thereby reducing the rebound rate of shotcrete from 20%-30% to less than 5%.

[0025] Specifically, the initiator can be selected from ammonium sulfate, sodium persulfate or potassium persulfate.

[0026] As an implementable method of the present application, the cross-linked body is a spatial network colloid including guar gum and xanthan gum, wherein the mass ratio of guar gum to xanthan gum is 3:2.

[0027] Specifically, guar gum is generally a white to light yellow-brown free-flowing powder, generally containing 75%-85% polysaccharides, 5%-6% protein, 2%-3% fiber and 1% ash. Xanthan gum is a carbohydrate, a complex polysaccharide produced by fermentation of Xanthomonas campestris. The cross-linked body of the present application is based on a mass ratio of 3:2 between guar gum and xanthan gum. The cross-linked body forms a colloid with a spatial network structure after cross-linking of the two polymer materials. The colloid can be adsorbed on the free water molecules in the concrete slurry and fix the mixing water in the concrete slurry, thereby increasing the viscosity of the concrete.

[0028] As an embodiment of the present application, the cross-linked body further comprises at least one of hydroxymethyl cellulose ether, hydroxyethyl cellulose ether and soluble starch ether. In order to further strengthen the spatial network structure of the cross-linked body, the present application adds hydroxymethyl cellulose ether, hydroxyethyl cellulose ether and soluble starch ether on the basis of guar gum and xanthan gum to form a stable spatial network structure.

[0029] As an implementation method of the present application, the polyether monomer includes one of isopentanol polyoxyethylene ether, 3-methylbut-3-enyl polyethylene glycol ether, 2-methylprop-2-enyl polyethylene glycol ether, ethylene glycol monovinyl polyoxyethylene ether and 4-hydroxybutyl vinyl polyoxyethylene ether.

[0030] Specifically, the polyether monomer of the present application has the function of a chain transfer agent, which plays a role in regulating the length of the polymerized molecular chain during the polymerization reaction. By reacting with the polymer chain, the intermediate free radicals formed in the polymerization reaction are transferred to themselves, thereby changing the length of the polymerized molecular chain, adjusting the rate of the polymerization reaction, and achieving the desired polymer properties. By adding the polyether monomer to the graft copolymerization reaction, short side chains can be further introduced into the crosslinked body, and the morphology of the polymer and the cured polymer can be regulated. Preferably, the polyether monomer is prenol polyoxyethylene ether.

[0031] As an implementation method of the present application, the small molecule monomers include at least two of acrylamide, acrylic acid, methacrylic acid, hydroxypropyl methacrylate and N,N-dimethylacrylamide.

[0032] Specifically, acrylamide, acrylic acid, methacrylic acid, hydroxypropyl methacrylate and N,N-dimethylacrylamide all have similar functional groups and similar molecular structures. The introduction of such small molecular monomers for graft copolymerization can introduce short side chains into the molecular structure of the thickener, and these short side chains contain hydroxyl, carboxyl, ester, amide and other groups. The oxygen atoms in the hydroxyl group will associate with the free water in the slurry and become bound water. The carboxyl group can adsorb cement particles, and the ester group and amide group can produce an associative bridging effect with the concrete slurry to form a stable spatial network structure. Therefore, the bridging effect between the thickener and the concrete particles can be further enhanced, and the bonding strength of the shotcrete can be improved.

[0033] As an implementable method of the present application, the preparation step of the thickener includes:

[0034] After heating the water to 55-65°C, add guar gum and xanthan gum, stir for 0.8-1.2h until dissolved, add polyether monomer, small molecule monomer and initiator, stir for 3-8min, let stand for 1.5-2.5h, then add 55-65°C water, stir for 8-12min, swell for 1.5-2.5h, while keeping the temperature at 55-65°C. After swelling, stir at 40-50°C for 10-14h, then add lignin solution and sodium hydroxide, stir for 10-20min to obtain the finished thickener.

[0035] In the present application, guar gum and xanthan gum are first swelled and dissolved in an aqueous solution to form a colloid with a spatial network structure, and then small molecule monomers are added, and graft copolymerization is carried out under the action of an initiator and a polyether monomer. Since short side chains are introduced into the molecular structure of the thickener, and these short side chains contain hydroxyl groups, carboxyl groups, ester groups, amide groups and the like, the copolymer prepared in the present application can further enhance the effective improvement of the cohesiveness of concrete.

[0036] As an implementable embodiment of the present application, the water retaining agent includes one of polyacrylamide and polyoxyethylene.

[0037] Since there are two kinds of water in the mixed concrete paste, free water and bound water, free water affects the fluidity of the fresh concrete paste, and bound water affects the hydration of the fresh concrete paste. When there is too much free water inside the fresh concrete paste, water segregation will occur. The water retaining agent can effectively reduce the fluidity of the fresh concrete paste, making the concrete particles inside the fresh concrete paste easier to gather and form aggregates, thereby improving the rheological properties of the concrete paste. Preferably, the water retaining agent is polyacrylamide.

[0038] As an implementable embodiment of the present application, the air entraining agent includes one of K12, AOS and AES.

[0039] Specifically, K12 is sodium dodecyl sulfate, AOS is sodium A-olefin sulfonate, and AES is sodium ethoxylated alkyl sulfate, all of which have certain emulsifying properties and can introduce air bubbles into the concrete paste, thereby playing a lubricating role, thereby improving the wrapping of concrete paste on concrete aggregates, making the produced concrete have better softness, thereby reducing the rebound rate of shotcrete during construction. Preferably, AOS is selected as the air entraining agent.

[0040] As an implementation method of the present application, the enhancer includes one of calcium formate, sodium carbonate and sodium sulfate.

[0041] Specifically, calcium formate can improve the strength and durability of concrete paste, increase the bonding force between concrete particles, and thus enhance the mechanical properties of concrete. At the same time, calcium formate can also adjust the setting time and hardening time of concrete paste, making it easier to construct; sodium carbonate can promote the reaction between concrete particles, thereby enhancing the strength and durability of concrete paste, and then improve the bonding strength of shotcrete; sodium sulfate can increase the viscosity and fluidity of concrete paste, making it easier to construct. The reinforcing agent can play the function of anchoring and enhancing the shotcrete, and the reinforcing agent is preferably sodium carbonate.

[0042] The embodiment of the present application also provides a method for preparing an anchoring elasticity reducing agent for shotcrete, comprising the following steps:

[0043] Add water into the reaction kettle, then add the water retaining agent, after it dissolves, then add the reinforcing agent, thickener and air entraining agent in sequence, stir for 30min-60min, and obtain the finished anchoring elasticity reducing agent.

[0044] The anchoring and elasticity reducing agent prepared in the present application is a liquid product. When used, it is added through a metering pump and stirred together with other components of concrete. When mixing concrete, there is no need to add additional ultrafine mineral admixtures to improve the cohesiveness of concrete. The anchoring and elasticity reducing agent can effectively enhance the bonding and anchoring effect between shotcrete and the base layer, and greatly reduce the rebound rate of shotcrete. It has the characteristics of low cost, high efficiency and simple operation.

[0045] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.

[0046] Example 1

[0047] An anchoring elasticity reducing agent for shotcrete is prepared by the following steps:

[0048] After heating 298.95 kg of deionized water to 60°C, add 0.63 kg of guar gum and 0.42 kg of xanthan gum, stir for 1 hour until dissolved, add 7.2 kg of isopentanol polyoxyethylene ether, 21.6 kg of acrylamide, 7.2 kg of acrylic acid and 0.18 kg of initiator ammonium persulfate, stir for 5 minutes, let stand for 2 hours, then add 2650 kg of deionized water at 60°C, stir for 10 minutes, swell for 2 hours, keep the temperature at 60°C, after swelling, stir at 45°C for 12 hours to dissolve the materials, then add 17 kg of sodium lignin solution and 9 kg of sodium hydroxide, stir for 15 minutes, and obtain a thickener;

[0049] Add 41 kg of water into the reactor, then add 0.25 kg of water-retaining agent polyacrylamide, and after dissolution, add 7.5 kg of reinforcing agent calcium formate, 50 kg of thickener and 0.25 kg of air entraining agent K12 in sequence. After stirring for 45 minutes, the finished anchoring elasticity reducing agent is obtained.

[0050] Example 2

[0051] An anchoring elasticity reducing agent for shotcrete is prepared by the following steps:

[0052] After heating 298.95 kg of deionized water to 55° C., add 0.63 kg of guar gum and 0.42 kg of xanthan gum, stir for 1.2 hours until dissolved, add 4 kg of 3-methylbut-3-enylpolyethylene glycol ether, 3.2 kg of 2-methylprop-2-enylpolyethylene glycol ether, 21.6 kg of acrylamide, 7.2 kg of acrylic acid and 0.18 kg of initiator sodium persulfate, stir for 3 minutes, let stand for 1.5 hours, then add 2650 kg of deionized water at 55° C., stir for 12 minutes, and swell for 2.5 hours while keeping the temperature at 55° C. After swelling, stir at 40° C. for 10 hours to dissolve the materials, then add 17 kg of sodium lignosulfate solution and 9 kg of sodium hydroxide, stir for 20 minutes, and obtain the finished thickener;

[0053] Add 29 kg of water into the reactor, then add 0.02 kg of water retaining agent polyoxyethylene. After dissolving, add 5 kg of reinforcing agent sodium carbonate, 40 kg of thickener and 0.05 kg of air entraining agent AOS in sequence. After stirring for 30 minutes, the finished anchoring elasticity reducing agent is obtained.

[0054] Example 3

[0055] An anchoring elasticity reducing agent for shotcrete is prepared by the following steps:

[0056] After heating 298.95 kg of deionized water to 65°C, add 0.63 kg of guar gum, 0.42 kg of xanthan gum, 0.03 kg of hydroxymethyl cellulose ether, 0.08 kg of hydroxyethyl cellulose ether and 0.04 kg of soluble starch ether, stir for 0.8 h until dissolved, add 1 kg of 2-methylprop-2-enyl polyethylene glycol ether, 3 kg of ethylene glycol monovinyl polyoxyethylene ether and 3.2 kg of 4-hydroxybutyl vinyl polyoxyethylene ether, 7.2 kg of methacrylic acid, 21.6 kg of hydroxypropyl methacrylate and 0.18 kg of initiator potassium persulfate, stir for 8 min, let stand for 2.5 h, then add 2650 kg of deionized water at 65°C, stir for 8 min, swell for 1.5 h, keep the temperature at 65°C, stir at 50°C for 14 h after swelling, dissolve the materials, add 17 kg of sodium lignosulfate solution and 9 kg of sodium hydroxide, stir for 10 min, and obtain the finished thickener;

[0057] Add 54.93 kg of water into the reactor, then add 0.5 kg of water retaining agent polyacrylamide, after dissolution, add 10 kg of reinforcing agent sodium sulfate, 60 kg of thickener and 0.5 kg of air entraining agent AES in sequence, stir for 60 minutes, and obtain the finished anchoring elasticity reducing agent.

[0058] Example 4

[0059] An anchoring elasticity reducing agent for shotcrete is prepared by the following steps:

[0060] After heating 298.95 kg of deionized water to 58°C, add 0.63 kg of guar gum, 0.42 kg of xanthan gum and 0.11 kg of hydroxyethyl cellulose ether, stir for 1.1 hours until dissolved, add 2 kg of 2-methylprop-2-enyl polyethylene glycol ether, 5.2 kg of ethylene glycol monovinyl polyoxyethylene ether, 21.6 kg of N,N-dimethylacrylamide, 7.2 kg of acrylic acid and 0.18 kg of initiator ammonium persulfate, stir for 4 minutes, let stand for 2.1 hours, then add 2650 kg of deionized water at 58°C, stir for 9 minutes, swell for 1.7 hours, keep the temperature at 58°C, stir at 48°C for 11 hours after swelling, then add 17 kg of sodium lignosulfate solution and 9 kg of sodium hydroxide, stir for 16 minutes, and obtain the finished thickener;

[0061] Add 44.22 kg of water into the reactor, then add 0.15 kg of water retaining agent polyoxyethylene. After dissolving, add 8 kg of reinforcing agent sodium sulfate, 45 kg of thickener and 0.3 kg of air entraining agent K12 in sequence. After stirring for 40 minutes, the finished anchoring elasticity reducing agent is obtained.

[0062] Example 5

[0063] An anchoring elasticity reducing agent for shotcrete is prepared by the following steps:

[0064] After heating 298.95 kg of deionized water to 55° C., add 0.63 kg of guar gum and 0.42 kg of xanthan gum, stir for 0.9 h until dissolved, add 4 kg of 3-methylbut-3-enyl polyethylene glycol ether, 3.2 kg of 4-hydroxybutylvinyl polyoxyethylene ether, 21.6 kg of acrylamide, 7.2 kg of acrylic acid and 0.18 kg of initiator ammonium persulfate, stir for 7 min, let stand for 2.2 h, then add 2650 kg of deionized water at 62° C., stir for 10 min, swell for 1.9 h, keep the temperature at 62° C., after swelling, stir at 47° C. for 11 h to dissolve the materials, then add 17 kg of sodium lignosulfate solution and 9 kg of sodium hydroxide, stir for 12 min, and obtain the finished thickener;

[0065] Add 34.83 kg of water into the reactor, then add 0.1 kg of polyacrylamide and 0.4 kg of polyoxyethylene. After dissolution, add 7 kg of reinforcing agent calcium formate, 55 kg of thickener and 0.35 kg of air entraining agent AOS in sequence. After stirring for 48 minutes, the finished anchoring elasticity reducing agent is obtained.

[0066] Comparative Example 1

[0067] Compared with Example 1, hydroxypropyl methylcellulose ether is used as the thickener, and the other steps remain unchanged.

[0068] Comparative Example 2

[0069] Compared with Example 1, maltodextrin is used as the thickener, and the other steps remain unchanged.

[0070] Experimental example

[0071] (I) Infrared spectroscopy testing of the thickener of the present application

[0072] The anchoring elasticity reducing agent prepared in Example 1 of the present application was subjected to infrared spectroscopy detection, and the detection spectrum was as follows: Figure 1 shown.

[0073] according to Figure 1 The absorption peak in the graph can be characterized. The molecular structure of the thickener contains hydroxyl, carboxyl, ester, amide and other groups, which can adsorb free water molecules, adsorb concrete particles, or produce an association and bridging effect with cement paste to form a stable spatial network structure, thereby enhancing the viscosity of the concrete.

[0074] (II) Testing the effect of the thickener of the present application on the rheological properties of concrete paste

[0075] The thickeners in Example 1 of the present application and Comparative Examples 1-2 were mixed with concrete paste respectively, and then the rheological properties and thixotropy of the fresh concrete paste were tested by a rheometer, and the rheological curve of the fresh concrete paste was fitted to obtain the yield stress and plastic viscosity of the fresh concrete paste, and a blank control group was set at the same time. The test results are shown in Table 1 below.

[0076] Table 1

[0077] Group Yield stress / Pa Plastic viscosity / Pa·s Blank control group 9.7 0.16 Comparative Example 1 42.91 0.89 Comparative Example 2 32.46 0.60 Example 1 66.38 1.78

[0078] As can be seen from Table 1, compared with the commonly used organic thickeners hydroxypropyl methylcellulose ether and maltodextrin, the thickener prepared in the present application can significantly improve the yield stress and plastic viscosity of the concrete slurry, indicating that the thickener of the present application is more effective in improving the rheological properties of the concrete slurry and can make the plastic viscosity of the concrete slurry larger.

[0079] (III) Testing the influence of the anchoring elasticity reducing agent of the present application on the rebound rate of shotcrete

[0080] 1 Experimental equipment:

[0081] 1.1 Mixer, volume greater than 1m 3 ;

[0082] 1.2 Spraying equipment;

[0083] 1.3 Plastic film, area 40m 2 -50m 2 ;

[0084] 1.4 Mechanical scale or electronic scale, with a measuring range of 500kg-3000kg and a graduation value of 200g-1000g;

[0085] 1.5 Samples to be tested: the anchoring elasticity reducing agent of Example 1, the anchoring elasticity reducing agent of Comparative Example 1 and the elasticity reducing agent from a certain factory on the market.

[0086] 2 Experimental steps:

[0087] 2.1 Cover the ground below the surface to be sprayed with plastic film for 40m 2 -50m 2 area;

[0088] 2.2 Mix the sample to be tested with concrete to form a concrete mixture (not less than 1m 3 ), sent to the spraying equipment, and the test will start after the spraying material is stable. The nozzle should maintain a 90° angle with the sprayed surface, the total spraying thickness is 80mm-120mm, and it is sprayed in two layers, each layer is 40mm-60mm thick. The spraying process must be continuous and uninterrupted, and the concrete in the hopper must be uniform at the beginning and end of the test;

[0089] 2.3 After the spraying is completed, the rebound material is collected from the plastic film and weighed;

[0090] 2.4 The mass percentage of the rebound material to the total sprayed mixture is the spray rebound rate. The total sprayed mixture should be deducted from the spray volume before the spray stabilizes. The test results are shown in Table 2 below.

[0091] Table 2

[0092]

[0093]

[0094] It can be seen from Table 2 that, compared with the anchoring elasticity reducing agent and the commercially available elasticity reducing agent in Comparative Example 1, the anchoring elasticity reducing agent of the present application can reduce the rebound rate of shotcrete from 20%-30% to less than 5%, and its rebound suppression effect on shotcrete is much higher than that of the anchoring elasticity reducing agent and the commercially available elasticity reducing agent in Comparative Example 1, and can achieve better rebound suppression effect with less dosage.

[0095] The above description is only an optional embodiment of the present application, and does not limit the patent scope of the present application. All equivalent structural transformations made by using the contents of the present application specification and drawings under the inventive concept of the present application, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present application.

Claims

1. An anchoring elasticity reducing agent for shotcrete, characterized in that: Calculated by mass percentage, it includes the following raw materials: Thickener 40%-60%, water retaining agent 0.02%-0.5%, air entraining agent 0.05%-0.5%, reinforcing agent 5%-10% and the balance water; The raw materials of the thickener include a cross-linker, a polyether monomer, a small molecule monomer and an initiator; The cross-linked body is a spatial network colloid comprising guar gum and xanthan gum, wherein the mass ratio of the guar gum to the xanthan gum is 3:2; the cross-linked body further comprises at least one of hydroxymethyl cellulose ether, hydroxyethyl cellulose ether and soluble starch ether; The polyether monomer includes one of isopentanol polyoxyethylene ether, 3-methylbut-3-enyl polyethylene glycol ether, 2-methylprop-2-enyl polyethylene glycol ether, ethylene glycol monovinyl polyoxyethylene ether and 4-hydroxybutyl vinyl polyoxyethylene ether; The small molecule monomers include at least two of acrylamide, acrylic acid, methacrylic acid, hydroxypropyl methacrylate and N,N-dimethylacrylamide; The preparation steps of the thickener include: After heating the water to 55-65°C, add guar gum and xanthan gum, stir for 0.8-1.2h until dissolved, add polyether monomer, small molecule monomer and initiator, stir for 3-8min, let stand for 1.5-2.5h, then add 55-65°C water, stir for 8-12min, swell for 1.5-2.5h, while keeping the temperature at 55-65°C. After swelling, stir at 40-50°C for 10-14h, then add lignin solution and sodium hydroxide, stir for 10-20min to obtain the finished thickener.

2. The anchoring elasticity reducing agent for shotcrete according to claim 1, characterized in that: The water retaining agent includes one of polyacrylamide and polyoxyethylene.

3. The anchoring elasticity reducing agent for shotcrete according to claim 1, characterized in that: The air entraining agent includes one of K12, AOS and AES.

4. The anchoring elasticity reducing agent for shotcrete according to claim 1, characterized in that: The enhancer includes one of calcium formate, sodium carbonate and sodium sulfate.

5. A method for preparing the anchoring elasticity reducing agent for shotcrete according to any one of claims 1 to 4, characterized in that: The following steps are involved: Add water into the reaction kettle, then add the water retaining agent, after it dissolves, then add the reinforcing agent, thickener and air entraining agent in sequence, stir for 30min-60min, and obtain the finished anchoring elasticity reducing agent.

Citation Information

Patent Citations

  • Tunnel engineering sprayed concrete resilience reducing agent and preparation method thereof