A carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber and preparation method thereof

By blending carboxylated boron nitride microspheres with epoxidized ethylene propylene teremer rubber in electronic equipment, a dynamic crosslinking network structure is solved, and the thermal interface material is insufficient and difficult to recover, achieving high thermal conductivity and repeatable processing effect, suitable for thermal management of electronic equipment.

CN118307893BActive Publication Date: 2024-11-08RONGFA NEW MATERIALS TECHNOLOGY DEVELOPMENT (QINGDAO) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410497378.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-11-08
Estimated Expiration
2044-04-24

AI Technical Summary

Technical Problem

The existing thermal interface materials are insufficient in electronic equipment and are difficult to recycle, which makes it difficult to solve the problem of heating of electronic equipment. At the same time, traditional rubber materials have scale challenges in the preparation of highly thermally conductive materials.

Method used

Carboxylated boron nitride microspheres are blended with epoxidized ethylene propylene teremer rubber to improve thermal conductivity and mechanical properties through dynamic crosslinking network structure, and the boron nitride microspheres are coated with dicarboxylic acid compounds to enhance dispersion Effects and repeatable processing properties.

Benefits of technology

It has achieved the significant improvement of the thermal conductivity and mechanical properties of composite rubber under low thermal filler content, and has given it excellent repeatable processing properties, and has the characteristics of green crosslinking and high thermal elastic thermal interface materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307893B_ABST
    Figure CN118307893B_ABST
Patent Text Reader

Abstract

The invention discloses a carboxylated boron nitride microsphere composite high thermal conductivity reinforced ethylene propylene diene monomer rubber and a preparation method thereof. The method is characterized in that firstly, ethylene propylene diene monomer rubber (EPDM) is subjected to epoxidation treatment under the condition of peroxy organic acid to introduce epoxy groups, then, by utilizing the property of sodium chloride (NaCl) evaporating and precipitating crystals in an aqueous solution, hexagonal boron nitride (h-BN) sheets are coated on NaCl crystals, hollow boron nitride microspheres (BNMS) are prepared by filtering, washing and assembling, and carboxylated boron nitride microspheres are prepared by coating with a dicarboxylic acid compound; finally, epoxidized ethylene propylene diene monomer rubber (eEPDM), carboxylated boron nitride microspheres and zinc salt are added to an open mill for blending, and hot pressing and vulcanization are performed after the mixing is completed to prepare a carboxylated boron nitride microsphere composite ethylene propylene diene monomer rubber composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermally conductive rubber, and in particular to a high thermally conductive reinforced EPDM rubber composited with carboxylated boron nitride microspheres and a preparation method thereof. Background Art

[0002] With the development of electronic products towards refinement, integration and high power, heat generation has become one of the main problems facing the electronics industry. In order to get rid of the dilemma of performance degradation of electronic equipment due to heat generation, the installation of cooling systems such as air cooling and water cooling was the main means of solving heat dissipation in the early days, but factors such as contact thermal resistance and diffusion thermal resistance were ignored. Therefore, precise heat diffusion and heat conduction between the heating point of electronic equipment and the cooling system have become an extremely critical step in the research and development and production of electronic equipment. Against this background, elastic thermal interface materials came into being.

[0003] Since the heating element and the heat sink are rough and cannot be 100% in contact, and there is air in the rest of the part (thermal conductivity is only 0.02 W / mK), the heat cannot be dissipated in time and accumulates on the surface of the components, resulting in reduced operating power of the electronic equipment and affecting its service life. Thermal interface materials can fully fill the gap between the heating element and the heat sink, effectively reduce the contact thermal resistance, and achieve rapid heat transfer. It is a key topic for research and solution in many industries and is of great significance to the development of related application fields. The thermal interface materials currently circulating on the market are mainly thermal conductive gel and thermal conductive silicone grease. Both can effectively fill the tiny gaps of electronic components, reduce contact thermal resistance, and effectively improve thermal conductivity. Because it needs to be cured during use and does not have thermoplastic processing properties, it is difficult to recycle after use, which will cause unnecessary waste. Therefore, designing a solid thermal interface material with high thermal conductivity and green recyclability has potential value in the field of electronic packaging.

[0004] Chinese patent CN202311824820.8 discloses a modified graphene oxide composite thermal conductive silicone gel and its preparation method, wherein graphene oxide is reduced by water-soluble cationic organic matter, and then mixed with silicone resin to finally obtain a thermal interface material with excellent mechanical properties and thermal conductivity. He et al., Tribology International, 2024, 193:109341, successfully prepared MXene-h-BN hybrid by introducing hexagonal boron nitride to the MXene surface using a simple thiol-ene click reaction to construct a unique layered structure. Layered MXene-h-BN has good lubricity, and h-BN can increase the strength and thermal conductivity of the MXene support skeleton. However, the production cost is high and cannot be mass-produced. Chinese patent CN202311735440.7 discloses a composite thermal conductive material based on a three-dimensional graphene structure, its preparation method and application, wherein polydimethylsiloxane is filled into the graphene skeleton and then cured to prepare a high thermal conductivity composite material. However, this method is only suitable for small molecules or prepolymer systems with low viscosity, and is not applicable to traditional rubber. Therefore, it is still challenging to use a method that is easy to scale to study and prepare high thermal conductivity elastic thermal conductive materials. Summary of the invention

[0005] The purpose of the present invention is to provide a preparation method of carboxylated boron nitride microspheres composite high thermal conductivity reinforced ethylene propylene diene monomer rubber in view of the shortcomings of the prior art. The method is characterized in that firstly, ethylene propylene diene monomer rubber (EPDM) is subjected to epoxidation treatment under the condition of peroxy organic acid to introduce epoxy groups, then, by utilizing the property of sodium chloride (NaCl) evaporating and precipitating crystals in an aqueous solution, hexagonal boron nitride (h-BN) sheets are coated on NaCl crystals, hollow boron nitride microspheres (BNMS) are prepared by filtering, washing and assembling, and carboxylated boron nitride microspheres are prepared by coating with dicarboxylic acid compounds; finally, epoxidized ethylene propylene diene monomer rubber (eEPDM), carboxylated boron nitride microspheres and zinc salt are added to an open mill for blending, and hot pressing and vulcanization are performed after the mixing is completed to prepare a carboxylated boron nitride microsphere composite ethylene propylene diene monomer rubber composite material. The reaction between the carboxyl group and the epoxy group on BNMS is used to form a dynamic cross-linked network. On the one hand, the formation of the dynamic cross-linked network structure is beneficial to improving the mechanical properties of EPDM rubber. On the other hand, an interfacial cross-linked structure is established between the thermally conductive boron nitride and the rubber matrix to improve the dispersion effect and reduce the interfacial phonon scattering. After hot pressing, it is more conducive to establishing a thermal conductive channel, and further improves the thermal conductivity of the composite rubber at a low thermal conductive filler content. At the same time, the formation of dynamic cross-linked bonds gives the composite rubber excellent repeatable processing performance and maintains high thermal conductivity.

[0006] The object of the present invention is achieved by the following technical scheme, wherein the raw material fractions are all mass fractions unless otherwise specified.

[0007] A carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber mainly composed of the following components:

[0008] EPDM 100 parts

[0009] Hexagonal boron nitride 5-15 parts

[0010] 3-10 parts of dicarboxylic acid compound

[0011] 1-4 parts zinc salt

[0012] Wherein, the dicarboxylic acid compound is any one of azelaic acid, sebacic acid, terephthalic acid, and maleic acid;

[0013] The zinc salt is any one of zinc chloride, zinc oxide, zinc acetate and zinc nitrate.

[0014] The preparation method of the carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber comprises the following steps:

[0015] Preparation of epoxidized EPDM rubber:

[0016] Dissolve 100 parts of EPDM in xylene to prepare an EPDM solution with a concentration of 2-10% by mass, add 1-5 parts of formic acid and 0.1-1 parts of Tween-80, stir at 50°C for 10 min, then add 5-20 parts of hydrogen peroxide dropwise within 10-30 min, stir to react to form peroxy organic acid, and form a uniform and stable emulsion system. After continuing the reaction for 3-8 h, precipitate the product in ethanol, wash it twice with distilled water, dry it in vacuum at 60°C for 8 h, and finally place it in a torque rheometer at 170 o C for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber (eEPDM).

[0017] Preparation of carboxylated boron nitride microspheres

[0018] 5-15 parts of hexagonal boron nitride (h-BN) were placed in a mixed solution of 100-800 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 h to make it uniformly dispersed. 0.1-0.3 parts of polyvinyl alcohol (PVA) and 5-10 parts of sodium chloride (NaCl) were dissolved in 90°C hot water. After complete dissolution, the above-mentioned uniformly dispersed h-BN suspension was poured in, and stirred and evaporated at 90°C to obtain NaCl crystals wrapped in h-BN, washed twice with cold water to remove NaCl, and then dried for 6 h to obtain boron nitride microspheres (BNMS). 3-10 parts of dicarboxylic acid compounds were dissolved in ethanol, BNMS was added and mixed and stirred for 30 min, filtered, washed and vacuum dried at 50°C for 3 h to obtain dicarboxylic acid-coated boron nitride microspheres.

[0019] Preparation of carboxylated boron nitride microspheres composite with high thermal conductivity reinforced EPDM rubber

[0020] 100 parts of eEPDM were added to an open mill and mixed at room temperature. After 5 minutes, the dicarboxylic acid-coated boron nitride microspheres prepared above were added and mixed evenly. Then 1-4 parts of zinc salt were added and mixed evenly. Finally, hot pressing was performed at 170°C and 15 MPa for 5-10 minutes to prepare carboxylated boron nitride microsphere composite EPDM rubber.

[0021] The present invention has the following advantages:

[0022] Thermally conductive fillers are poorly dispersed in the rubber matrix, making it difficult to exert their intrinsic high thermal conductivity, and large amounts of filling will also reduce the elasticity and mechanical properties of the rubber. The present invention assembles two-dimensional boron nitride sheets into boron nitride microspheres, and coats them with dicarboxylic acid compounds, and then covalently crosslinks them with epoxidized EPDM rubber. The assembled boron nitride microspheres form more oriented thermal conductive pathways in the EPDM rubber, and the surface of the thermally conductive boron nitride establishes a dynamic crosslinking network with the epoxidized EPDM rubber, thereby improving the dispersion effect and reducing interface phonon scattering. At the same time, the dynamic crosslinking characteristics give the composite rubber good mechanical properties and repeatable processing performance, thereby realizing the preparation of green crosslinked high thermal conductivity elastic thermal interface materials. The preparation method is simple, the conditions are mild, and the thermal conductivity is significantly improved, which has certain advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope image of the microstructure of boron nitride microspheres.

[0024] Figure 2 Schematic diagram of the thermal conductivity mechanism of composite rubber. DETAILED DESCRIPTION

[0025] The present invention is further described below through specific examples. It should be noted that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make non-essential improvements and adjustments to the present invention based on the contents of the present invention described above. Example 1

[0026] 100 parts of EPDM were dissolved in xylene to prepare a 2% mass fraction EPDM solution, 2 parts of formic acid and 0.1 parts of Tween-80 were added, and stirred at 50°C for 10 min. Then, 5 parts of hydrogen peroxide were added dropwise within 10 min, and stirred to react to form peroxy organic acid, forming a uniform and stable emulsion system. After continuing the reaction for 3 h, the product was precipitated in ethanol, washed twice with distilled water, and vacuum dried at 60°C for 8 h. Finally, it was placed in a torque rheometer and heated at 170 oC for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber (eEPDM).

[0027] 5 parts of hexagonal boron nitride (h-BN) were placed in a mixed solution of 100 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 hours to make it uniformly dispersed. 0.1 parts of polyvinyl alcohol (PVA) and 5 parts of sodium chloride (NaCl) were dissolved in 90℃ hot water. After complete dissolution, the above-mentioned uniformly dispersed h-BN suspension was poured in, and stirred and evaporated at 90℃ to obtain NaCl crystals wrapped in h-BN. The NaCl was washed twice with cold water to remove NaCl, and then dried for 6 hours to obtain boron nitride microspheres (BNMS). 3 parts of azelaic acid were dissolved in ethanol, BNMS was added and mixed and stirred for 30 minutes, filtered, washed and vacuum dried at 50℃ for 3 hours to obtain azelaic acid-coated boron nitride microspheres.

[0028] 100 parts of eEPDM were added to an open mill and mixed at room temperature. After 5 minutes, azelaic acid-coated boron nitride microspheres were added and mixed evenly. Then 1 part of zinc chloride was added and mixed evenly. Finally, carboxylated boron nitride microsphere composite EPDM rubber was prepared by hot pressing at 170°C and 15 MPa for 6 minutes. The tensile strength of the composite EPDM rubber was 2.35MPa, the elongation at break was 384%, the thermal conductivity was 1.273 W / mK, the tensile strength recovery rate was 83% after three repeated processing, and the thermal conductivity was 1.106 W / mK. Example 2

[0029] 100 parts of EPDM were dissolved in xylene to prepare a 4% mass fraction EPDM solution, 2 parts of formic acid and 0.2 parts of Tween-80 were added, and stirred at 50°C for 10 min. Then, 8 parts of hydrogen peroxide were added dropwise within 15 min, and stirred to react to form peroxy organic acid, forming a uniform and stable emulsion system. After continuing the reaction for 4 h, the product was precipitated in ethanol, washed twice with distilled water, and vacuum dried at 60°C for 8 h. Finally, it was placed in a torque rheometer and heated at 170 o C for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber (eEPDM).

[0030] 8 parts of hexagonal boron nitride (h-BN) were placed in a mixed solution of 400 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 hours to make it uniformly dispersed. 0.2 parts of polyvinyl alcohol (PVA) and 6 parts of sodium chloride (NaCl) were dissolved in 90℃ hot water. After complete dissolution, the above-mentioned uniformly dispersed h-BN suspension was poured in, and stirred and evaporated at 90℃ to obtain NaCl crystals wrapped in h-BN. The NaCl was washed twice with cold water to remove NaCl, and then dried for 6 hours to obtain boron nitride microspheres (BNMS). 5 parts of sebacic acid were dissolved in ethanol, BNMS was added and mixed and stirred for 30 minutes, filtered, washed and vacuum dried at 50℃ for 3 hours to obtain sebacic acid-coated boron nitride microspheres.

[0031] 100 parts of eEPDM were added to an open mill and mixed at room temperature. After 5 minutes, sebacic acid-coated boron nitride microspheres were added and mixed evenly. Then 2 parts of zinc oxide were added and mixed evenly. Finally, carboxylated boron nitride microsphere composite EPDM rubber was prepared by hot pressing at 170°C and 15 MPa for 6 minutes. The tensile strength of the composite EPDM rubber was 2.82MPa, the elongation at break was 417%, the thermal conductivity was 1.696 W / mK, the tensile strength recovery rate was 86% after three repeated processing, and the thermal conductivity was 1.236 W / mK. Example 3

[0032] 100 parts of EPDM were dissolved in xylene to prepare a 6% mass fraction EPDM solution, 3 parts of formic acid and 0.3 parts of Tween-80 were added, and stirred at 50°C for 10 min. Then, 10 parts of hydrogen peroxide were added dropwise within 25 min, and stirred to react to form peroxy organic acid, forming a uniform and stable emulsion system. After continuing the reaction for 5 h, the product was precipitated in ethanol, washed twice with distilled water, and vacuum dried at 60°C for 8 h. Finally, it was placed in a torque rheometer and heated at 170 o C for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber (eEPDM).

[0033] 10 parts of hexagonal boron nitride (h-BN) were placed in a mixed solution of 600 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 h to make it uniformly dispersed. 0.2 parts of polyvinyl alcohol (PVA) and 8 parts of sodium chloride (NaCl) were dissolved in 90°C hot water. After complete dissolution, the above-mentioned uniformly dispersed h-BN suspension was poured in, and NaCl crystals wrapped in h-BN were obtained while stirring and evaporating at 90°C. The NaCl was washed twice with cold water to remove NaCl, and then dried for 6 h to obtain boron nitride microspheres (BNMS). 8 parts of maleic acid were dissolved in ethanol, BNMS was added and mixed and stirred for 30 min, filtered, washed and vacuum dried at 50°C for 3 h to obtain maleic acid-coated boron nitride microspheres.

[0034] 100 parts of eEPDM were added to an open mill and mixed at room temperature. After 5 minutes, maleic acid-coated boron nitride microspheres were added and mixed evenly. Then 3 parts of zinc acetate were added and mixed evenly. Finally, carboxylated boron nitride microsphere composite EPDM rubber was prepared by hot pressing at 170°C and 15 MPa for 8 minutes. The tensile strength of the composite EPDM rubber was 3.11MPa, the elongation at break was 401%, and the thermal conductivity was 2.140 W / mK. After repeated processing three times, the tensile strength recovery rate was 88%, and the thermal conductivity was 1.733 W / mK. Example 4

[0035] 100 parts of EPDM were dissolved in xylene to prepare a 10% mass fraction EPDM solution, 5 parts of formic acid and 1 part of Tween-80 were added, and stirred at 50°C for 10 min. Then, 15 parts of hydrogen peroxide were added dropwise within 30 min, and stirred to react to form peroxy organic acid, forming a uniform and stable emulsion system. After continuing the reaction for 8 h, the product was precipitated in ethanol, washed twice with distilled water, and vacuum dried at 60°C for 8 h. Finally, it was placed in a torque rheometer and heated at 170 o C for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber (eEPDM).

[0036] 12 parts of hexagonal boron nitride (h-BN) were placed in a mixed solution of 800 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 h to make it uniformly dispersed. 0.3 parts of polyvinyl alcohol (PVA) and 10 parts of sodium chloride (NaCl) were dissolved in 90°C hot water. After complete dissolution, the above-mentioned uniformly dispersed h-BN suspension was poured in, and the h-BN-wrapped NaCl crystals were obtained while stirring and evaporating at 90°C. The NaCl crystals were washed twice with cold water to remove the NaCl, and then dried for 6 h to obtain boron nitride microspheres (BNMS). 10 parts of terephthalic acid were dissolved in ethanol, BNMS was added and mixed and stirred for 30 min, and terephthalic acid-coated boron nitride microspheres were obtained by suction filtration, washing and vacuum drying at 50°C for 3 h.

[0037] 100 parts of eEPDM were added to an open mill and mixed at room temperature. After 5 minutes, terephthalic acid-coated boron nitride microspheres were added and mixed evenly. Then 4 parts of zinc nitrate were added and mixed evenly. Finally, carboxylated boron nitride microsphere composite EPDM rubber was prepared by hot pressing at 170°C and 15 MPa for 10 minutes. The tensile strength of the composite EPDM rubber was 2.839 MPa, the elongation at break was 372%, the thermal conductivity was 2.380 W / mK, the tensile strength recovery rate was 79% after three repeated processing, and the thermal conductivity was 1.914 W / mK.

[0038] In summary, the addition of carboxylated boron nitride microspheres in the embodiment of the present invention has an enhancing effect on the mechanical properties and thermal conductivity of epoxidized EPDM rubber, while achieving repeated processing and maintaining excellent mechanical strength and thermal conductivity after repeated processing.

[0039] The above embodiments describe the specific contents of the present invention in detail, but the present invention is not limited to the embodiments, and those skilled in the art can make equivalent substitutions, which should be included in the protection scope of the present invention.

Claims

1. A carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber, characterized in that The main raw materials of the rubber are composed of the following components, calculated by weight: EPDM 100 parts Hexagonal boron nitride 5-15 parts 3-10 parts of dicarboxylic acid compound 1-4 parts zinc salt Wherein, the dicarboxylic acid compound is any one of azelaic acid, sebacic acid, terephthalic acid, and maleic acid; The zinc salt is any one of zinc chloride, zinc oxide, zinc acetate and zinc nitrate; The method for preparing a carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber comprises the following steps: S1: Preparation of epoxidized EPDM rubber: Dissolve 100 parts of EPDM in xylene to prepare an EPDM solution with a concentration of 2-10% by mass, add 1-5 parts of formic acid and 0.1-1 parts of Tween-80, stir at 50°C for 10 min, then add 5-20 parts of hydrogen peroxide dropwise within 10-30 min, stir to react to form peroxy organic acid, and form a uniform and stable emulsion system. After continuing the reaction for 3-8 h, precipitate the product in ethanol, wash it twice with distilled water, dry it in vacuum at 60°C for 8 h, and finally place it in a torque rheometer at 170 o C for 5 min to completely remove the peroxy organic acid and obtain epoxidized ethylene propylene diene monomer rubber eEPDM; S2: Preparation of carboxylated boron nitride microspheres 5-15 parts of hexagonal boron nitride (h-BN) are placed in a mixed solution of 100-800 parts of isopropanol and water in a volume ratio of 1:1, and ultrasonicated for 2 hours to make it uniformly dispersed, 0.1-0.3 parts of polyvinyl alcohol PVA and 5-10 parts of sodium chloride NaCl are dissolved in 90°C hot water, and after they are completely dissolved, the above-mentioned uniformly dispersed h-BN suspension is poured into it, and stirred and evaporated at 90°C to obtain NaCl crystals wrapped in h-BN, washed twice with cold water to remove NaCl, and then dried for 6 hours to obtain boron nitride microspheres BNMS; 3-10 parts of a dicarboxylic acid compound are dissolved in ethanol, added to BNMS, mixed and stirred for 30 minutes, filtered, washed and vacuum dried at 50°C for 3 hours to obtain dicarboxylic acid-coated boron nitride microspheres; S3: Preparation of carboxylated boron nitride microspheres composite with high thermal conductivity reinforced EPDM rubber 100 parts of eEPDM were added into an open mill and mixed at room temperature. After 5 minutes, the dicarboxylic acid-coated boron nitride microspheres prepared above were added and mixed evenly. Then 1-4 parts of zinc salt were added and mixed evenly. Finally, hot pressing was performed at 170°C and 15 MPa for 5-10 minutes to prepare carboxylated boron nitride microsphere composite high thermal conductivity reinforced EPDM rubber.