A kind of preparation method of clay-based cat litter

By using materials such as highly active silicon sources and nano-silver ions after depolymerizing natural clay, combined with microwave processing technology, clay-based cat litter with long-term sterilization and high adsorption properties is prepared, which solves the problem of environmental emissions and environmental pollution of existing cat litter. The problem of single material is achieved, and environmentally friendly and efficient cat litter preparation is achieved.

CN118318740BActive Publication Date: 2024-10-01YANBIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410757423.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Existing cat litter has shortcomings in terms of functional synthesis and non-polluting environmental emissions after use, and is made from a single material, which may cause pain, bad taste and easy breeding of bacteria.

Method used

The highly active silicon source after the depolymerization of natural clay is used to replace traditional cat litter synthetic materials. It is combined with nano-silver ions and graphene to give long-term sterilization performance through a step-by-step microwave treatment process, and uses clay-based nano-hectorite and tea residue powder. To enhance water absorption and adsorption properties to form clay-based cat litter.

Benefits of technology

It achieves long-term sterilization of cat litter, environmental protection and no pollution emissions to the natural environment, reduces synthesis costs and raw material pollution, and at the same time gives the cat litter a natural taste and high adsorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118318740B_ABST
    Figure CN118318740B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a clay-based cat litter, wherein the weight percentage of the raw materials is 50-70% of a clay-based active silicon source, 5-10% of a clay-based nano-hectorite, 0.1-10% of tea residue powder, 0.001-0.005% of nano silver ions, 0.1-1% of graphene, and the remainder is ionized water. Thanks to the high activity of the clay-based active silicon source and the uniqueness of the synthesis method, the present invention relates to the technical field of cat litters, the method of the present invention is simple and convenient, the prepared clay-based cat litter eliminates the use of chemical raw materials, greatly reduces the preparation cost of traditional cat litter synthesis, and has both sterilization and can be naturally discarded. The remarkable characteristics provide a new way for the high value-added development and comprehensive utilization of clay resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cat litter, and in particular to a method for preparing clay-based cat litter. Background Art

[0002] Cat litter is an object used by cats to bury feces and urine. It has good water absorption and is usually used together with a cat litter box (or cat toilet). The most important progress in cat culture is the use of cat litter. Early cat litters were mainly non-condensing cat litters, mainly for collecting cat feces. In recent years, with the continuous improvement and progress of science and technology and the improvement of living standards, the cat litter industry has also made great progress, and different types of cat litters such as condensed litter, wood litter, crystal litter, bentonite litter, etc. have been born.

[0003] The cat litter produced by the prior art is generally made of pulp as raw material, which is beaten into small particles to simulate sand and provide water absorption. In recent years, there have also been technical reports on the use of silica gel, corn flour, starch, and plant fiber as adsorption and synthetic raw materials for the preparation of industrial cat litter. In the process of making cat litter, it is usually possible to add chemical products such as antibacterial agents, deodorants, and preservatives to give it certain functionality (such as bactericidal properties, deodorizing properties, preservatives, dust prevention, etc.), which has led to a series of new methods for preparing cat litter. For example, the prior art CN202211490404.4 discloses an antibacterial and deodorizing cat litter and a method for preparing it, that is, adding a cationic bactericide (such as alkyl trimethyl quaternary ammonium salt, dialkyl dimethyl quaternary ammonium salt and guanidine salt polymer, etc.) and a deodorant (unsaturated fatty acid zinc salts including ricinoleic acid zinc, undecylenic acid zinc and itaconate zinc) to the cat litter to achieve its bactericidal and deodorizing functions. Prior art CN202410043932.8 discloses a cat litter containing graphene and a preparation method thereof, that is, by adding graphene and grapefruit peel to the cat litter, it can achieve the high adsorption and high antibacterial properties of the cat litter, and at the same time prevent pets from eating it. Prior art CN202311619748.5 discloses a new type of environmentally friendly straw cat litter and a preparation method thereof, that is, rice straw powder is mixed with poplar fluff pulp, and calcium carbonate powder, lavender powder and other materials are added to prepare cat litter, so as to solve the problems of single materials and methods for making cat litter, pain when cats step on it, bad taste of cat litter, alkaline pH value, easy breeding of bacteria and sticking to the bottom. Prior art CN202311757408.9 discloses a pet cat litter deodorant and antibacterial agent based on bamboo extract and its application, that is, by adding bamboo extract and modified zeolite to give cat litter antibacterial and deodorizing functions. However, the existing technology has always been insufficient in terms of the functional synthesis of cat litter and whether it can be directly discharged into the natural environment after use. In order to further increase the additional functions of cat litter and enable the waste cat litter after use to be discharged into the natural environment without pollution, we proposed a method for preparing clay-based cat litter. Summary of the invention

[0004] The present invention aims to overcome the shortcomings of the prior art and provide a method for preparing a clay-based cat litter. In the present invention, a highly active silicon source (i.e., a clay-based active silicon source) produced after the depolymerization of natural clay is used to replace the main material for synthesizing traditional cat litter. At the same time, the nanosilver ions are fixed by means of the active groups remaining after the depolymerization of natural clay, and a secondary identification is performed by means of a step-by-step microwave treatment process to give it a long-lasting bactericidal performance. In this process, graphene is added to enhance the microwave absorption efficiency of the material, reduce energy consumption, and increase the specific surface area. At the same time, the topological structure remaining after the depolymerization of natural clay is reconstructed in situ to prepare clay-based lithium soapstone as a water-absorbing material and a bonding material. In addition, tea residue powder is added to further improve the adsorption performance of the cat litter and give it a natural taste of grass and trees. The above technologies are combined, that is, the application technology of the present invention: a method for preparing a clay-based cat litter.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for preparing a clay-based cat litter. The cat litter comprises the following raw materials in parts by weight: 50-70% of a clay-based active silicon source, 5-10% of a clay-based nano-lithium laponite, 0.1-10% of tea residue powder, 0.001-0.005% of nano-silver ions, 0.1-1% of graphene, and the balance is ionized water.

[0007] The preparation method is as follows:

[0008] Step 1. Mix the clay-based nano-hectorite with water and stir with a stirrer at a stirring speed of 1000-7000 rpm, a stirring temperature of 25-40 ° C, and a stirring time of 0.5-3 h. The obtained raw material is recorded as material 1;

[0009] Step 2. Mix the clay-based active silicon source, nanosilver ions, graphene, and water with a stirrer. After mixing evenly, transfer the resulting mixed solution to a microwave digestion tank. Place the microwave digestion tank in a microwave digestion instrument for reaction. The reaction conditions are: reaction temperature 100-160°C, irradiation frequency: 100w irradiation 10s, 150w irradiation 10s, 200w irradiation 10s, 250w irradiation 10s, 350w irradiation 10s, stop 10s, irradiation cycle 10-30, after the reaction is completed, take out, the resulting product is recorded as material 2;

[0010] Step 3. Mix material 1, material 2, and tea residue powder, stir evenly, take out and extrude granules, and after granulation, place them in a constant temperature oven for drying. The drying temperature is 85-90°C, the drying time is 6-12h; the granulator power is 100-150 W, the granulation temperature is 60-70°C, and the cat litter particle size obtained by granulation is 1-3 mm.

[0011] The method for preparing the clay-based active silicon source is as follows:

[0012] S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;

[0013] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay: acid solution = 1g: 2.5ml-5 ml;

[0014] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated at a certain temperature according to specific irradiation conditions, specifically the irradiation temperature of 110-200 ℃, the irradiation cycle is 30;

[0015] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;

[0016] Furthermore, the natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite;

[0017] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L;

[0018] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.

[0019] Furthermore, the irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s.

[0020] The method for preparing the clay-based nano-hectorite is as follows:

[0021] A. Mix the lithium source, magnesium source, and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir thoroughly, transfer to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 9-12;

[0022] B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The specific conditions are that the irradiation temperature is 110-180 °C and the irradiation cycle is 10-30;

[0023] C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-lithium laponite.

[0024] Furthermore, in step A, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two.

[0025] Furthermore, the irradiation cycle mentioned in step B is specifically each cycle of 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.

[0026] The graphene has a flake lateral distance of 1-2 um and a carbon-oxygen ratio of 4-7.

[0027] The nano silver ions have a diameter of 10 nm.

[0028] The tea residue powder is obtained by drying and crushing the tea waste produced after drinking tea. The specific drying conditions are 50-70°C and the drying time is 12-24 hours. The dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain tea residue powder; further, in the process of preparing clay-based cat litter, the tea residue selected is a mixture of one or more of jasmine tea, Tieguanyin tea, and Longjing tea residue.

[0029] Compared with the prior art, the advantages of the present invention are as follows:

[0030] First of all, in terms of synthetic raw materials, this method is completely different from the main raw materials for the preparation of cat litter at present. The silicon source we use is the silicon source produced by acid depolymerization of natural clay as the synthetic raw material (i.e., clay-based active silicon source), which to a certain extent alleviates the problem of upper-end pollution of synthetic raw materials caused by the use of silicon-containing chemicals (such as silica gel), and also reduces the synthetic cost of cat litter. In addition, for the process of obtaining clay-based active silicon sources, we originally proposed and adopted a superimposed composite process of a solid-phase method and a microwave progressive irradiation method, that is, firstly, the natural clay is separated from the acid solution in a microwave digestion tank, and the acid solution is heated and evaporated by microwave irradiation to produce acid vapor, which then reacts with the natural clay. The advantage of this is that, on the one hand, low-concentration acid solution can play the effect of high-concentration acid solution, effectively improving the use efficiency of acid solution, and at the same time, it can also be recycled multiple times by appropriately adding a small amount of acid solution. In addition, a large number of high-value elements, such as aluminum and potassium, can be present in the acid solution, which can be effectively enriched through the above process to facilitate the high added value utilization of clay minerals.

[0031] Secondly, under the microwave progressive irradiation environment, affected by the solid-phase system, the natural clay powder is directly irradiated by microwaves. Since different chemical bonds receive microwaves differently, they can be directly activated, and the chemical bond activation and broken parts will be consistent. This is not only the reason why the natural clay can be depolymerized without the high-temperature activation step in the technology of the present invention. At the same time, the broken chemical bonds can better combine with the nano silver ions firmly and evenly through chemical interactions. Through the microwave action, the loading mode of the nano silver ions can be further identified (under this condition, the nano silver ions can only be combined by chemical means, and physical adsorption is eliminated), so that the bactericidal effect of the cat litter is maximized while avoiding excessive use of nano silver ions.

[0032] Again, in the present invention, nano lithium soapstone (clay-based active silicon source as the synthetic raw material of nano lithium soapstone) and tea residue powder are used as cat litter adsorption units and odor modification units, which not only eliminates the addition of chemicals (chemical synthetic flavors) again, but also further makes the process of synthesizing cat litter greener. It is noted again that because the clay-based active silicon source we obtained has ultra-high activity, if the traditional microwave synthesis method is directly used, due to the uncontrollable heat supply, the crystal nucleus will grow rapidly through the Oswald reaction after generation, and the lithium soapstone obtained will show the characteristics of chaotic crystal size distribution. However, when using microwave progressive irradiation, since the chemical bonds broken by the silicon raw material are consistent, and the heat supply method is regularized, it is conducive to the synthesis of nano lithium soapstone with uniform morphology, which is extremely beneficial for the preparation of clay cat litter.

[0033] Finally, since only pollution-free components are used in the production process of cat litter, and no additional chemical components are added, after the cat litter is used, it can be discharged into the natural environment as solid fertilizer, avoiding the environmental pollution problem caused by the discharge of discarded cat litter. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0035] Figure 1 This is the XRD diagram of the clay-based active silicon source in Example 1.

[0036] Figure 2 This is the XRD diagram of clay-based nano-lithium laponite in Example 1.

[0037] Figure 3This is an actual picture of the S1 material produced by mixing the clay-based nano-hectorite and water described in Example 1.

[0038] Figure 4 This is the SEM image of the clay-based nano-hectorite described in Example 1.

[0039] Figure 5 This is the TEM image of the clay-based nano-lithium laponite described in Example 8.

[0040] from Figure 1 It can be seen that the clay-based active silicon source product presents an amorphous structure, indicating that its inherent crystal structure has been completely depolymerized into active species suitable for synthesizing hectorite.

[0041] Figure 2 This is the XRD diagram of the product nano-hectorite in Example 1. Based on its diffraction peak, it can be determined that the synthesized product is nano-hectorite, which further proves that it is synthesized from a clay-based active silicon source.

[0042] Figure 3 This is an actual picture of the S1 material produced by mixing the clay-based nano-hectorite and water recorded in Example 1 (the picture shows 100 ml of water mixed with 0.3 g of clay-based nano-hectorite), which can prove that it has excellent water absorption and gelation ability.

[0043] Figure 4 The clay-based nano-heterostilbene obtained under the experimental environment of Example 1 presents a relatively uniform flaky morphology at the nanoscale.

[0044] Figure 5 The clay-based nano-heterostilbene obtained under the experimental environment of Example 8 presents a relatively uniform flaky morphology at the nanoscale. DETAILED DESCRIPTION

[0045] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification: Example

[0046] This embodiment provides a method for preparing clay-based cat litter, and the specific steps of the method are as follows:

[0047] The cat litter comprises the following raw materials in parts by weight: 70% of clay-based active silicon source, 10% of clay-based nano-lithium laponite, 0.1% of tea residue powder, 0.005% of nano-silver ions, 1% of graphene, and the balance is ionized water.

[0048] The preparation method is as follows:

[0049] Step 1. Mix the clay-based nano-hectorite with water and stir with a stirrer at a stirring speed of 7000 rpm, a stirring temperature of 40° C., and a stirring time of 0.5 h. The obtained raw material is recorded as material 1;

[0050] Step 2. The clay-based active silicon source, nanosilver ions, graphene and water are mixed with a stirrer. After being mixed evenly, the obtained mixed solution is transferred to a microwave digestion tank, and the microwave digestion tank is placed in a microwave digestion instrument for reaction. The reaction conditions are: reaction temperature 160° C., irradiation cycle 10, after the reaction is completed, it is taken out, and the obtained product is recorded as material 2;

[0051] Furthermore, the specific irradiation parameters of each irradiation cycle are: 100w irradiation for 10s, 150w irradiation for 10s, 200w irradiation for 10s, 250w irradiation for 10s, 350w irradiation for 10s, and stop for 10s.

[0052] Step 3. Mix material 1, material 2, and tea residue powder, stir evenly, take out and extrude granules, and after granulation, place them in a constant temperature oven for drying. The drying temperature is 85°C, the drying time is 12h; the granulator power is 150 W, the granulation temperature is 70°C, and the cat litter particle size obtained by granulation is 1 mm.

[0053] The method for preparing the clay-based active silicon source is as follows:

[0054] S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;

[0055] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay: acid solution = 1g:2.5ml;

[0056] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 200 ° C, and the irradiation cycle is 30;

[0057] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;

[0058] Furthermore, the natural clay in step S1 is rectorite;

[0059] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L;

[0060] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.

[0061] Furthermore, the irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s.

[0062] The clay-based nano-hectorite preparation method is as follows:

[0063] A. Mix the lithium source, magnesium source, and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir thoroughly, transfer to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 12;

[0064] B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The specific irradiation conditions are: irradiation temperature is 180 °C and irradiation cycle is 10;

[0065] C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-lithium laponite.

[0066] Furthermore, in step A, the lithium source is lithium carbonate; and the magnesium source is magnesium hydroxide.

[0067] Furthermore, the irradiation cycle mentioned in step B is specifically each cycle of 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.

[0068] The graphene has a flake lateral distance of 2 um and a carbon-oxygen ratio of 7.

[0069] The nano silver ions have a diameter of 10 nm.

[0070] The tea residue powder is obtained by drying and crushing the tea waste produced after drinking jasmine tea. The specific drying conditions are 70°C and the drying time is 24 hours. The dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain tea residue powder; further, in the process of preparing clay-based cat litter, the tea residue selected is jasmine tea residue.

[0071] The rest of Example 2 is the same as Example 1, except that the cat litter is prepared by comprising the following raw materials in parts by weight: 60% clay-based active silicon source, 5% clay-based nano-lithium laponite, 10% tea residue powder, 0.002% nano-silver ions, 0.5% graphene, and the balance is ionized water.

[0072] The rest of Example 3 is the same as Example 1, except that the cat litter is prepared by comprising the following raw materials in parts by weight: 60% clay-based active silicon source, 8% clay-based nano-lithium laponite, 5% tea residue powder, 0.003% nano-silver ions, 0.5% graphene, and the balance is ionized water.

[0073] The rest of Example 4 is the same as Example 1, except that the cat litter particle size is 2 mm.

[0074] The rest of Example 5 is the same as Example 1, except that the power of the granulator in step S3 is 100 W, and the tea residues used are Longjing tea residues.

[0075] The rest of Example 6 is the same as Example 1, except that the natural clay in step S1 is kaolin.

[0076] The rest of Example 7 is the same as Example 1, except that the natural clay in step S1 is montmorillonite.

[0077] The rest of Example 8 is the same as Example 1, except that in step A, the lithium source is lithium fluoride and the magnesium source is magnesium chloride.

[0078] The rest of Example 9 is the same as Example 1, except that the tea residue powder is obtained by drying and crushing the tea waste produced after drinking Tieguanyin tea.

[0079] The rest of Example 10 is the same as Example 1, except that the tea residue powder is obtained by drying and crushing the tea waste generated after drinking Longjing tea.

[0080] Experimental data:

[0081] serial number Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Water absorption (%) 743 755 743 748 750 728 759 742 748 739 Moisture determination (%) 0.4 0.5 0.4 0.5 0.3 0.2 0.2 0.4 0.6 0.4

[0082] Water absorption test:

[0083] 1. Place the standard sieve in a stainless steel pan filled with water, making the water level about 5 mm above the sieve, and soak for 10 seconds.

[0084] 2. Take out the wet standard sieve from the water container, place it at a 30° angle for 5 minutes, and then weigh the wet standard sieve.

[0085] 3. Accurately weigh 10.0 g of the cat litter sample obtained under the conditions of each embodiment that has been dried to constant weight at 105°C ± 5°C, place it in a wet standard sieve, and spread the sample evenly on about 1 / 2 of the sieve surface.

[0086] 4. Slowly immerse the standard sieve and the sample into the water container. During the water absorption process, make sure the water surface always submerges the cat litter sample.

[0087] 5. After absorbing water for 5 minutes, slowly take out the standard sieve containing the wet sample from the water container, place it at a 30° angle for 10 minutes, and then weigh it on a balance.

[0088] The water absorption rate X of the sample is expressed as mass fraction (%) and is calculated according to the formula X=(BAC) / C*100.

[0089] Where: A is the mass of the empty wet sieve, in grams (g); B is the mass of the sample after wet sieve and water absorption, in grams (g); C is the mass of the sample, in grams (g). The arithmetic mean of the results of three parallel measurements is taken as the measurement result.

[0090] Moisture determination:

[0091] Weigh 10g of each cat litter prepared under the conditions of each example, place it in a constant temperature oven at 105±2℃, and dry it under atmospheric pressure until constant weight. The lost weight is water. The ratio of the mass of water contained in the sample to the mass of the sample represents the water content in the sample.

[0092] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing clay-based cat litter, characterized in that: The cat litter is prepared by comprising the following raw materials in parts by weight: 50-70% clay-based active silicon source, 5-10% clay-based nano-hectorite, 0.1-10% tea residue powder, 0.001-0.005% nano silver ions, 0.1-1% graphene, and the balance is ionized water; The preparation method is as follows: Step 1. Mix the clay-based nano-hectorite with water, stir with a stirrer, the stirring speed is 1000-7000 rpm, the stirring temperature is 25-40 ° C, the stirring time is 0.5-3 h, and the obtained raw material is recorded as material 1; Step 2. The clay-based active silicon source, nanosilver ions, graphene and water are mixed with a stirrer. After being mixed evenly, the obtained mixed solution is transferred to a microwave digestion tank, and the microwave digestion tank is placed in a microwave digestion instrument for reaction. The reaction conditions are: irradiation temperature 100-160°C, irradiation cycle 10-30, after the reaction is completed, it is taken out, and the obtained product is recorded as material 2; The specific irradiation parameters of each irradiation cycle are: 100w irradiation for 10s, 150w irradiation for 10s, 200w irradiation for 10s, 250w irradiation for 10s, 350w irradiation for 10s, and stop for 10s; Step 3. Mix material 1, material 2, and tea residue powder, stir evenly, take out and extrude granules. After granulation, place it in a constant temperature oven and dry it at a temperature of 85-90°C for 6-12h. The power of the granulator is 100-150 W, the granulation temperature is 60-70°C, and the cat litter particle size obtained by granulation is 1-3 mm. The method for preparing the clay-based active silicon source is as follows: S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder; S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay: acid solution = 1g: 2.5ml-5ml; S3, loading the microwave digestion vessel prepared in step S2 into a microwave digestion instrument, and irradiating the microwave digestion vessel according to specific irradiation conditions, specifically, the irradiation temperature is 110-200° C., and the irradiation cycle is 30; S4, taking out the microwave digestion tank after microwave irradiation, filtering the solid product until it is neutral, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is the clay-based active silicon source; The natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite; The acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L; In step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium; The irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s; The clay-based nano-hectorite preparation method is as follows: A. Mix the lithium source, magnesium source and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir them thoroughly, transfer them to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 9-12; B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The specific conditions are that the irradiation temperature is 110-180 ℃ and the irradiation cycle is 10-30; C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-hectorite; In step A, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two; The irradiation cycle mentioned in step B is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.

2. A method for preparing a clay-based cat litter according to claim 1, characterized in that: The graphene has a flake lateral distance of 1-2 um and a carbon-oxygen ratio of 4-7.

3. according to the preparation method of a kind of clay-based cat litter described in claim 1, described nano silver ion, its diameter is 10nm.

4. According to the method for preparing a clay-based cat litter as claimed in claim 1, the tea residue powder is obtained by drying and crushing tea waste generated after drinking tea, the specific drying conditions are 50-70°C, the drying time is 12-24 h, the dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain the tea residue powder; in the process of preparing the clay-based cat litter, the tea residue selected is a mixture of one or more of jasmine tea, Tieguanyin tea, and Longjing tea residue.