Polyurethane three-proof paint and preparation method thereof

Through the cross-linking reaction of aqueous polyurethane emulsion, alkyl ketone dimer and film-forming resin, combined with 1,6-hexanediol diacrylate, the problem of polyurethane triple anti-paint cracking is solved, and the crack resistance strength and durability are improved. Extends service life and is environmentally friendly.

CN118325457BActive Publication Date: 2024-11-15HUIZHOU JUXIN CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410604738.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-11-15
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Polyurethane triple-proof paint is prone to cracking in actual applications, affecting the appearance quality and protective performance of the coating, resulting in a shortening of service life.

Method used

The three-dimensional network structure is formed by cross-linking reaction of aqueous polyurethane emulsion, alkyl ketone dimer and film-forming resin, which increases the adhesion and flexibility of the three-proof paint and the substrate, and is formed by 1,6-hexanediol diacrylate. Elastic chain segments, combined with catalysts to promote reactions, improve crack resistance and durability.

Benefits of technology

It significantly improves the crack resistance strength and durability of polyurethane triple-proof paint, reduces cracking phenomenon, enhances adhesion and flexibility with the substrate, extends service life, and compared with traditional solvent-based paint, water-based polyurethane emulsion is harmless Volatile substances, environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004841618910000061
    Figure BDA0004841618910000061
  • Figure BDA0004841618910000071
    Figure BDA0004841618910000071
Patent Text Reader

Abstract

The present application relates to the field of coating technology, and specifically discloses a polyurethane three-proof paint and a preparation method thereof. A polyurethane three-proof paint comprises the following raw materials in parts by weight: 10-15 parts of aqueous polyurethane emulsion, 2-5 parts of film-forming resin, 0.1-0.5 parts of catalyst, 1-3 parts of 1,6-hexanediol diacrylate, and 2-5 parts of alkyl ketene dimer, wherein the aqueous polyurethane emulsion is prepared from diphenylmethane diisocyanate, polyoxypropylene glycol, 2-hydroxyethyl methacrylate phosphate, and a cross-linking agent; its preparation method is: vacuum heating the aqueous polyurethane emulsion to 110-120°C, adding film-forming resin and 1,6-hexanediol diacrylate, stirring and mixing, cooling to 60-80°C, adding a catalyst and alkyl ketene dimer while stirring, and mixing evenly. The composition of the present application can be used in the fields of electronics, electrical appliances, automobiles, and aerospace, and has the advantage of good crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of coatings, and more specifically, to a polyurethane conformal coating and a preparation method thereof. Background Art

[0002] Polyurethane conformal coating is a commonly used high-performance coating. Due to its excellent high and low temperature resistance, insulation, moisture resistance, leakage resistance, shock resistance, dust resistance, corrosion resistance, anti-aging performance and corona resistance, it is widely used in the protection and decoration of electronics, electrical appliances, automobiles, aerospace and other fields. However, in practical applications, polyurethane conformal coating faces a serious problem, that is, the paint surface is prone to cracking. This cracking problem not only seriously affects the appearance quality of the coating, but may also cause the failure of the coating's protective performance, thereby affecting its service life.

[0003] Therefore, developing a simple, efficient and low-cost method for preparing polyurethane conformal coatings to improve their anti-cracking properties is of great practical significance for solving the cracking problem in the application of polyurethane conformal coatings. Summary of the invention

[0004] In order to improve the crack resistance of polyurethane conformal coating, the present application provides a polyurethane conformal coating and a preparation method thereof.

[0005] In the first aspect, the present application provides a polyurethane conformal paint, which adopts the following technical solution:

[0006] A polyurethane conformal paint comprises the following raw materials in parts by weight:

[0007] The invention discloses a waterborne polyurethane emulsion comprising 10-15 parts of waterborne polyurethane emulsion, 2-5 parts of film-forming resin, 0.1-0.5 parts of catalyst, 1-3 parts of 1,6-hexanediol diacrylate and 2-5 parts of alkyl ketene dimer. The waterborne polyurethane emulsion is prepared from diphenylmethane diisocyanate, polyoxypropylene glycol, 2-hydroxyethyl methacrylate phosphate and a crosslinking agent.

[0008] By adopting the above technical solution, since alkyl ketene dimer is an active chemical substance, it can react chemically with other components in the coating to form a stronger chemical bond, which helps to improve the adhesion between the three-proof paint and the substrate, so that the three-proof paint fits the substrate more closely and reduces the possibility of cracking. In addition, the alkyl ketene dimer can participate in the cross-linking reaction of polyurethane and other resin materials to form a three-dimensional network structure, enhance the internal bonding force of the three-proof paint, and further improve the crack resistance and durability of the three-proof paint. The addition of 1,6-hexanediol diacrylate can increase the flexibility of the three-proof paint, form elastic segments in the three-proof paint, and make the three-proof paint less likely to crack when subjected to external stress. At the same time, it can react with the alkyl ketene dimer to form a stronger chemical bond with the substrate, and work together to improve the flexibility of the three-proof paint, which helps to alleviate the stress concentration caused by deformation of the substrate or temperature change, and improves the durability and crack resistance of the three-proof paint.

[0009] Optionally, the aqueous polyurethane emulsion is prepared by the following steps:

[0010] Take diphenylmethane diisocyanate and polyoxypropylene glycol, mix them, heat them to 90-100° C. and react for 2-3 hours, add a crosslinking agent and 2-hydroxyethyl methacrylate phosphate, control the temperature at 80-90° C., continue to react for 1-2 hours, and after the reaction is completed, cool to 60-70° C., add triethylamine, and add deionized water under high-speed stirring conditions for emulsification to obtain the aqueous polyurethane emulsion.

[0011] By adopting the above technical scheme, diphenylmethane diisocyanate and polyoxypropylene glycol undergo polymerization reaction to form a prepolymer, and a cross-linking agent is added later to help form a network structure, and 2-hydroxyethyl methacrylate phosphate is added to introduce a phosphate group to the polyurethane chain segment, and triethylamine is added for neutralization reaction, so that the hydroxyl and amino groups in the polyurethane form a more stable salt, thereby improving the stability of the polyurethane emulsion, and deionized water is added under high-speed stirring conditions to emulsify and form an aqueous polyurethane emulsion. The prepared polyurethane emulsion has hydroxyl groups that can better adsorb with alkyl ketene dimers, thereby improving the compatibility of alkyl ketene dimers in three-proof paints, thereby improving the durability of the three-proof paints and preventing the three-proof paints from cracking. The addition of phosphate groups not only makes the three-proof paint have good corrosion resistance and weather resistance, but also improves its adhesion and compatibility with other raw materials, and better resists cracking and peeling.

[0012] Optionally, the addition ratio of the diphenylmethane diisocyanate, polyoxypropylene glycol, 2-hydroxyethyl methacrylate phosphate and the cross-linking agent is 6-7.2:6:1:2-3.

[0013] By adopting the above technical solution, the diphenylmethane diisocyanate is used as the main reaction component to react with polyoxypropylene glycol to generate a polymer with a cross-linked structure. The addition of a cross-linking agent can further enhance the cross-linking structure, thereby improving the toughness and crack resistance of the three-proof paint. Therefore, the amount of the cross-linking agent added will affect the performance of the prepared three-proof paint. The polyurethane prepared by controlling the cross-linking agent within a reasonable range has good crack resistance after curing.

[0014] Optionally, the cross-linking agent is any one of trimethylolpropane or castor oil.

[0015] By adopting the above technical scheme, the particle size and viscosity of the prepared polyurethane are relatively small. At the same time, hydroxyl groups are introduced into the polyurethane chain segments to improve the binding ability with alkyl ketene dimer, thereby improving the compatibility between the polyurethane emulsion and other raw materials, and improving the firmness of the binding between the raw materials, thereby improving the durability and crack resistance of the three-proof paint.

[0016] Optionally, the film-forming resin is acrylic resin.

[0017] By adopting the above technical solution, acrylic resin can reduce the internal stress caused by the difference in compatibility between different components and the shrinkage occurring during the curing process, improve the compatibility between components and curing shrinkage, and further improve the crack resistance of the coating.

[0018] Optionally, the raw materials further include 2-3 parts of dipropylene glycol diacrylate.

[0019] By adopting the above technical scheme, the acrylate group of dipropylene glycol diacrylate can undergo a cross-linking reaction with the unsaturated group in the polyurethane, further strengthening the three-dimensional network structure, improving the cross-linking density and cohesion of the three-proof paint, thereby improving the crack resistance and durability of the three-proof paint, and dipropylene glycol diacrylate has good elasticity and can absorb and release stress, thereby reducing the stress caused by temperature changes or curing shrinkage, reducing the tendency of cracks and microcracks to form, and further improving the crack resistance of the three-proof paint.

[0020] Optionally, the catalyst is dibutyltin dichloride.

[0021] By adopting the above technical solution, in the preparation process of polyurethane conformal coating, the selection of catalyst is crucial to the quality of the product. Dibutyltin dichloride can promote the reaction between the components, making the product more uniform and dense, thereby improving the protective performance and durability of the coating.

[0022] In a second aspect, the present application provides a method for preparing a polyurethane conformal coating, using the following technical solution:

[0023] A method for preparing a polyurethane conformal coating comprises the following steps:

[0024] The aqueous polyurethane emulsion is vacuum-heated to 110-120° C., a film-forming resin and 1,6-hexanediol diacrylate are added and stirred thoroughly, the temperature is lowered to 60-80° C., a catalyst and an alkyl ketene dimer are added while stirring and mixed uniformly to obtain the polyurethane conformal coating.

[0025] In summary, this application has the following beneficial effects:

[0026] 1. Since the present application adopts water-based polyurethane emulsion, alkyl ketene dimer and film-forming resin to form a three-dimensional network structure through cross-linking reaction, on the one hand, the adhesion between the three-conformal paint and the substrate is improved, so that the three-conformal paint fits the substrate more closely; on the other hand, the flexibility of the three-conformal paint is improved, so that the three-conformal paint is not easy to crack when subjected to stress, thereby improving the crack resistance of the three-conformal paint.

[0027] 2. In the present application, it is preferred that a phosphate group is introduced when preparing the waterborne polyurethane emulsion, which improves the corrosion resistance of the surface of the three-proof paint while improving the adhesion between the three-proof paint and the substrate, so that the prepared three-proof paint can better resist cracking and peeling.

[0028] 3. 1,6-hexanediol diacrylate is added in this application, which can adhere to the network structure to form elastic segments, improve the flexibility of the three-proof paint, thereby improving the ability of the three-proof paint to resist stress, thereby improving the anti-cracking performance of the three-proof paint.

[0029] 4. This application uses water-based polyurethane emulsion to prepare three-proof paint. Compared with traditional solvent-based paint, water-based polyurethane emulsion does not contain harmful volatile organic compounds (VOC) and is environmentally friendly. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0032] Alkyl ketene dimer was purchased from Zhonghe Chemical (Shandong) Co., Ltd., model: ZH1840; polyoxypropylene glycol was purchased from Jiangsu Xinsu New Materials Co., Ltd., model: 25322-69-4; alkyd resin was purchased from Hanpin Paint (Shandong) Co., Ltd., brand: 456313513.

[0033] Preparation examples of raw materials and / or intermediates

[0034] Preparation Example 1

[0035] A waterborne polyurethane emulsion, the preparation of which comprises the following steps:

[0036] Take 15kg of diphenylmethane diisocyanate and 15kg of polyoxypropylene glycol, mix them, heat to 95°C and stir to react for 3h, add 2.5kg of cross-linking agent and 5kg of 2-hydroxyethyl methacrylate phosphate, control the temperature at 85°C, continue to react for 2h, cool to 70°C, add triethylamine to neutralize into salt, add 20kg of deionized water under high-speed stirring at 3000r / min for emulsification, and obtain the aqueous polyurethane emulsion, wherein the cross-linking agent is pentaerythritol.

[0037] Preparation Example 2

[0038] A waterborne polyurethane emulsion, the preparation of which comprises the following steps:

[0039] 16.5 kg of diphenylmethane diisocyanate and 15 kg of polyoxypropylene glycol were mixed, heated to 90° C. and stirred for reaction for 3 hours, 2.5 kg of a cross-linking agent and 6.25 kg of 2-hydroxyethyl methacrylate phosphate were added, the temperature was controlled at 90° C., the reaction was continued for 2 hours, the mixture was cooled to 65° C., triethylamine was added to neutralize the mixture into salt, 20 kg of deionized water was added to emulsify the mixture under high-speed stirring at 3000 r / min, and the aqueous polyurethane emulsion was obtained, wherein the cross-linking agent was pentaerythritol.

[0040] Preparation Example 3

[0041] A waterborne polyurethane emulsion, the preparation of which comprises the following steps:

[0042] 18 kg of diphenylmethane diisocyanate and 15 kg of polyoxypropylene glycol were mixed, heated to 100 ° C and stirred for reaction for 3 hours, 2.5 kg of a cross-linking agent and 7.5 kg of 2-hydroxyethyl methacrylate phosphate were added, the temperature was controlled at 80 ° C, and the reaction was continued for 2 hours. After that, the mixture was cooled to 60 ° C and triethylamine was added to neutralize the mixture into salts. Under the condition of high-speed stirring at 3000 r / min, 20 kg of deionized water was added for emulsification to obtain the aqueous polyurethane emulsion, wherein the cross-linking agent was pentaerythritol.

[0043] Preparation Example 4

[0044] A waterborne polyurethane emulsion, which is different from Preparation Example 1 in that the crosslinking agent used in this Preparation Example is trimethylolpropane.

[0045] Preparation Example 5

[0046] A water-based polyurethane emulsion, which is different from Preparation Example 1 in that the cross-linking agent used in this Preparation Example is castor oil.

[0047] Preparation Example 6

[0048] A waterborne polyurethane emulsion, the preparation of which comprises the following steps:

[0049] Take 15 kg of diphenylmethane diisocyanate and 15 kg of polyoxypropylene glycol, mix them, heat to 95° C. and stir to react for 3 hours, add 2.5 kg of a cross-linking agent, control the temperature at 85° C., continue to react for 2 hours, cool to 70° C., add triethylamine to neutralize into salt, add 20 kg of deionized water under high-speed stirring at 3000 r / min to emulsify, and obtain the aqueous polyurethane emulsion, wherein the cross-linking agent is pentaerythritol.

[0050] Example

[0051] Example 1

[0052] A polyurethane conformal paint, the preparation of which comprises the following steps:

[0053] 10 kg of waterborne polyurethane emulsion was evacuated (gauge pressure -0.1 MPa) and heated to 110° C., 5 kg of film-forming resin and 2 kg of 1,6-hexanediol diacrylate were added and stirred thoroughly, and the temperature was lowered to 70° C., and 0.1 kg of catalyst and 5 kg of alkyl ketene dimer were added while stirring and mixed evenly to obtain the polyurethane conformal paint; the waterborne polyurethane emulsion was prepared in Preparation Example 1, the film-forming resin was acrylic resin, and the catalyst was dibutyltin dichloride.

[0054] Example 2

[0055] A polyurethane conformal paint, the preparation of which comprises the following steps:

[0056] 12.5 kg of waterborne polyurethane emulsion was evacuated (gauge pressure -0.1 MPa) and heated to 115° C., 2 kg of film-forming resin and 3 kg of 1,6-hexanediol diacrylate were added and stirred thoroughly, the temperature was lowered to 80° C., 0.3 kg of catalyst and 3.5 kg of alkyl ketene dimer were added while stirring and mixed evenly to obtain the polyurethane conformal paint; the waterborne polyurethane emulsion was prepared in Preparation Example 1, the film-forming resin was acrylic resin, and the catalyst was dibutyltin dichloride.

[0057] Example 3

[0058] A polyurethane conformal paint, the preparation of which comprises the following steps:

[0059] 15 kg of waterborne polyurethane emulsion was evacuated (gauge pressure -0.1 MPa) and heated to 120° C., 3.5 kg of film-forming resin and 1 kg of 1,6-hexanediol diacrylate were added and stirred thoroughly, the temperature was lowered to 60° C., 0.5 kg of catalyst and 2 kg of alkyl ketene dimer were added while stirring and mixed evenly to obtain the polyurethane conformal paint; the waterborne polyurethane emulsion was prepared in Preparation Example 1, the film-forming resin was acrylic resin, and the catalyst was dibutyltin dichloride.

[0060] Example 4

[0061] A polyurethane conformal paint, which is different from Example 1 in that the aqueous polyurethane emulsion used in this example is prepared in Preparation Example 2.

[0062] Example 5

[0063] A polyurethane conformal paint, which is different from Example 1 in that the aqueous polyurethane emulsion used in this example is prepared in Preparation Example 3.

[0064] Example 6

[0065] A polyurethane conformal paint, which is different from Example 1 in that the aqueous polyurethane emulsion used in this example is prepared in Preparation Example 4.

[0066] Example 7

[0067] A polyurethane conformal paint, which is different from Example 1 in that the aqueous polyurethane emulsion used in this example is prepared in Preparation Example 5.

[0068] Example 8

[0069] A polyurethane conformal paint, which is different from Example 1 in that the film-forming resin used in this example is an alkyd resin.

[0070] Example 9

[0071] A polyurethane conformal paint, which is different from Example 1 in that this embodiment further includes 2 kg of dipropylene glycol diacrylate, and the preparation includes the following steps:

[0072] 10 kg of waterborne polyurethane emulsion was evacuated (gauge pressure -0.1 MPa) and heated to 110° C., 5 kg of film-forming resin, 2 kg of 1,6-hexanediol diacrylate and 2 kg of dipropylene glycol diacrylate were added and stirred thoroughly, and the temperature was lowered to 70° C., and 0.1 kg of catalyst and 5 kg of alkyl ketene dimer were added while stirring and mixed uniformly to obtain the polyurethane conformal paint; the waterborne polyurethane emulsion was prepared in Preparation Example 1, the film-forming resin was acrylic resin, and the catalyst was dibutyltin dichloride.

[0073] Example 10

[0074] A polyurethane conformal paint, which is different from Example 9 in that 3 kg of dipropylene glycol diacrylate is added in this example.

[0075] Comparative Example

[0076] Comparative Example 1

[0077] A polyurethane conformal coating, which is different from Example 1 in that no alkyl ketene dimer is added in this comparative example.

[0078] Comparative Example 2

[0079] A polyurethane conformal paint, which is different from Example 1 in that the aqueous polyurethane emulsion used in this comparative example is prepared in Preparation Example 6.

[0080] Comparative Example 3

[0081] A polyurethane conformal coating, which is different from Example 1 in that 1,6-hexanediol diacrylate is not added in this comparative example.

[0082] Performance testing

[0083] Detection method / test method

[0084] Adhesion test: The test method refers to GB / T5210-2006 "Pull-off adhesion test for paints and varnishes";

[0085] Corrosion resistance: Test acid resistance using the immersion method, referring to GB / T9274-1988 "Determination of resistance of paints and varnishes to liquid media";

[0086] Crack resistance: Use an impact resistance tester to measure the impact strength of the prepared three-proof paint with reference to GB / T1732-1993 "Determination of impact resistance of paint film", so as to indirectly judge its crack resistance.

[0087] Table 1 Test results

[0088]

[0089]

[0090] Combining Example 1 and Comparative Example 1 with Table 1, it can be seen that the experimental data of Example 1 are better than those of Comparative Example 1, indicating that the addition of alkyl ketene dimer is beneficial to cooperate with other raw materials in the conformal coating to form a network structure, helping to improve the adhesion between the conformal coating and the substrate, thereby improving the anti-cracking performance of the conformal coating.

[0091] Combining Example 1 and Comparative Example 2 with Table 1, it can be seen that the experimental data of Example 1 are better than those of Comparative Example 2, indicating that the polyurethane emulsion prepared in the present application can more tightly connect the alkyl ketene dimer, improve the compatibility between the raw materials, and greatly improve the adhesion of the conformal coating to the substrate. Better resistance to cracking and peeling.

[0092] Combining Example 1 and Comparative Example 3 with Table 1, it can be seen that the experimental data of Example 1 are better than those of Comparative Example 3, indicating that the addition of 1,6-hexanediol diacrylate can greatly improve the flexibility of the three-conformal coating, making the three-conformal coating less likely to crack when subjected to external stress, and can also undergo esterification reaction with alkyl ketene dimer, further improving the adhesion between the three-conformal coating and the substrate, thereby improving the impact strength of the three-conformal coating.

[0093] It can be seen from Examples 1-7 and Table 1 that the experimental data of Examples 6-7 are better than those of Examples 1-5, indicating that when pentaerythritol is selected as a cross-linking agent, adding it to the polymer will greatly increase the degree of cross-linking of the molecular chain, thereby increasing the degree of cross-linking of the emulsion, increasing the viscosity, and making the emulsion difficult to emulsify, resulting in an increase in the particle size of the emulsion, resulting in reduced flexibility of the prepared three-proof paint, and weaker resistance to cracks. When trimethylolpropane or castor oil is used as a cross-linking agent, it has a long and soft molecular chain segment, which reduces the cohesive force of the three-proof paint and improves the anti-cracking performance of the three-proof paint.

[0094] Combining Example 1 with Example 8 and Table 1, it can be seen that the experimental data of Example 1 are better than those of Example 8, indicating that the selection of acrylic resin as the film-forming resin can improve the compatibility between the raw materials of the three-proof coating, reduce the internal stress caused by shrinkage and other phenomena generated during the curing process, and further improve the crack resistance of the coating.

[0095] Combining Example 1 with Examples 9-10 and Table 1, it can be seen that the experimental data of Examples 9-10 are better than those of Example 1, indicating that the addition of dipropylene glycol diacrylate to the raw materials can strengthen the three-dimensional network structure formed in the conformal coating, increase the crosslinking density and cohesion of the conformal coating, and thus improve the anti-cracking performance of the conformal coating.

[0096] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A polyurethane conformal paint, characterized in that: The composition comprises the following raw materials in parts by weight: 10-15 parts of waterborne polyurethane emulsion, 2-5 parts of film-forming resin, 0.1-0.5 parts of catalyst, 1-3 parts of 1,6-hexanediol diacrylate and 2-5 parts of alkyl ketene dimer. The waterborne polyurethane emulsion is prepared from diphenylmethane diisocyanate, polyoxypropylene glycol, 2-hydroxyethyl methacrylate phosphate and a crosslinking agent; the film-forming resin is an acrylic resin; the crosslinking agent is any one of trimethylolpropane and castor oil; the addition ratio of diphenylmethane diisocyanate, polyoxypropylene glycol, 2-hydroxyethyl methacrylate phosphate and the crosslinking agent is 6-7.2:6:1:2-3.

2. The polyurethane conformal coating according to claim 1, characterized in that: The aqueous polyurethane emulsion is prepared by the following steps: Take diphenylmethane diisocyanate and polyoxypropylene glycol, mix them, heat them to 90-100° C. and react for 2-3 hours, add a crosslinking agent and 2-hydroxyethyl methacrylate phosphate, control the temperature at 80-90° C., continue to react for 1-2 hours, and after the reaction is completed, cool to 60-70° C., add triethylamine, and add deionized water under high-speed stirring conditions for emulsification to obtain the aqueous polyurethane emulsion.

3. The polyurethane conformal coating according to claim 1, characterized in that: The raw materials also include 2-3 parts of dipropylene glycol diacrylate.

4. The polyurethane conformal coating according to claim 1, characterized in that: The catalyst is dibutyltin dichloride.

5. A method for preparing a polyurethane conformal coating according to any one of claims 1, 2, and 4, characterized in that: The steps include: The aqueous polyurethane emulsion is vacuum-heated to 110-120° C., a film-forming resin and 1,6-hexanediol diacrylate are added and stirred thoroughly, the temperature is lowered to 60-80° C., a catalyst and an alkyl ketene dimer are added while stirring and mixed uniformly to obtain the polyurethane conformal coating.