A water-based paint containing nanomaterials and preparation method thereof
By using modified polyurethane and modified nanoalumina in water-based paint, combined with specific stirring methods, the problem of corrosion and flame retardant effect of water-based paint during long-term use is solved, and significant improvement in antibacterial and flame retardant performance is achieved. , enhance its anti-corrosion protection capability.
Patent Information
- Application Number
- CN202410579151.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-11
AI Technical Summary
Existing water-based paints are easily corroded during long-term use, and the flame retardant effect is reduced, resulting in poor protection effect and lack effective antibacterial and flame retardant properties.
20-30 parts by weight of aqueous polyurethane dispersion, 10-15 parts by weight of modified polyurethane, 5-8 parts by weight of modified nanoalumina, 5-15 parts by weight of acrylic resin, 8-12 parts by weight of poly Vinyl alcohol and 1-2 parts by weight of pure water, prepare nanomaterial water-containing water paint by specific stirring methods, and improve flame retardant and antibacterial effects using modified polyurethane and modified nanoalumina phosphorus elements and quaternary ammonium salt groups. .
It significantly improves the antibacterial and flame retardant properties of water-based paint, and enhances its durability and effect in anticorrosion protection.
Smart Images

Figure BDA0004833329290000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a water-based paint containing nano materials and a preparation method thereof. Background Art
[0002] Water-based paint refers to a paint that uses water as a solvent or a dispersion medium. Water-based paint is harmless to the human body and has little pollution to the environment. It is widely used in various anti-corrosion protection aspects such as automobiles, ships, machinery manufacturing, railways, bridges, boilers, steel structures, etc. However, it will be corroded during long-term use, and the flame retardant effect will be reduced, resulting in a deterioration in the protective effect. How to avoid this phenomenon is the key to solving the problem; for example, the document "Synthesis of DOPO-containing thiazole derivatives and their flame retardant application in epoxy resins" reports the synthesis of DOPO-based flame retardants, which have good flame retardant effects; inspired by this, in this application, DOPO-based flame retardants are cited to synthesize water-based paints with antibacterial and flame retardant properties. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a water-based paint containing nanomaterials and a preparation method thereof, which has good antibacterial and flame retardant effects.
[0005] (II) Technical solution
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a water-based paint containing nano materials, comprising the following weight components: 20-30 weight parts of water-based polyurethane dispersion, 10-15 weight parts of modified polyurethane, 5-8 weight parts of modified nano alumina, 5-15 weight parts of acrylic resin, 8-12 weight parts of polyvinyl alcohol, and 1-2 weight parts of pure water.
[0007] Preferably, the preparation method of the modified polyurethane is:
[0008] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 40-60° C. for 2-4 hours, and then adding 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, continuing the reaction for 20-25 hours, cooling, filtering and drying after completion to obtain a phosphorus-containing modified thiazole;
[0009] (2) adding 2,2-bis(bromomethyl)-1,3-propanediol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, stirring evenly, and then adding 4-6 mol / L sodium hydroxide aqueous solution, reflux reaction at 40-60° C. for 12-18 hours. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0010] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst, introducing nitrogen protection, and then adding a phosphorus-containing chain extender. After the reaction is completed, cooling and discharging the material to obtain a modified polyurethane.
[0011] Preferably, the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in (1) is 1.1-1.2:1:1.1-1.3.
[0012] Preferably, the mass ratio of 2,2-bis(bromomethyl)-1,3-propanediol to phosphorus-modified thiazole in (2) is 1:1.2-1.6.
[0013] Preferably, the mass ratio of the polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender in (3) is 1.2-1.5:1:0.02-0.04:0.5-0.9.
[0014] Preferably, the preparation method of the modified nano-alumina is:
[0015] S1. Add nano-alumina to a mixed solvent of ethanol and deionized water, disperse by ultrasonication, stir evenly, then continue to add γ-aminopropyltriethoxysilane, react at 70-90°C for 10-12h, centrifuge after the reaction, wash and dry to obtain amino-alumina nano-alumina;
[0016] S2. Adding the amino nano-alumina and p-hydroxybenzaldehyde to the reactor, reacting at 70-80°C for 6-8h, adding diethyl phosphite, reacting at 70-80°C for 6-10h, distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0017] S3. Add phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stir evenly, heat in a water bath at 60-80°C, add 2,3-epoxypropyltrimethylammonium chloride under constant pressure, react for 5-8h, and then remove the solvent by reduced pressure distillation, wash and dry to obtain modified nano-alumina.
[0018] Preferably, the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane in S1 is 1:1.2-1.4.
[0019] Preferably, the mass ratio of the amino nano-alumina, p-hydroxybenzaldehyde and diethyl phosphite in S2 is 0.9-1.4:1:1.1-1.2.
[0020] Preferably, the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride in S3 is 1:1.1-1.3.
[0021] Preferably, the preparation method of the water-based paint containing nanomaterials comprises the following steps: adding water-based polyurethane dispersion, modified polyurethane, modified nano-alumina, acrylic resin, polyvinyl alcohol and pure water into a stirrer, stirring evenly at a stirring speed of 600-800 r / min and a stirring time of 10-15 min to obtain a water-based paint containing nanomaterials.
[0022] (III) Beneficial technical effects
[0023] The invention obtains water-based paint containing nano materials by adding water-based polyurethane dispersion, modified polyurethane, modified nano aluminum oxide, acrylic resin, polyvinyl alcohol and pure water into a stirrer and stirring them evenly.
[0024] The phosphorus element contained in the modified polyurethane and modified nano-alumina has a good flame retardant effect, and the nano-alumina itself has a good flame retardant effect; at the same time, the quaternary ammonium salt group contained in the modified nano-alumina also has a synergistic antibacterial effect.
[0025] During the stirring and mixing process, the hydroxyl groups in the modified nano-alumina will react with the terminal isocyanate in the modified polyurethane, resulting in cross-linking between them, which increases the compatibility between the two and makes them more evenly distributed in the water-based paint, thereby improving its antibacterial and flame retardant effects. DETAILED DESCRIPTION
[0026] Example 1
[0027] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 40° C. for 2 hours, and then continuing to add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1.1:1:1.1, and continuing the reaction for 20 hours. After the reaction is completed, cooling, suction filtering and drying are performed to obtain phosphorus-containing modified thiazole;
[0028] (2) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to phosphorus-modified thiazole is 1:1.2, stirring evenly, and then adding 4 mol / L sodium hydroxide aqueous solution, reflux reaction at 40° C. for 12 h. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0029] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst thereto, introducing nitrogen protection, and then adding a phosphorus-containing chain extender, wherein the mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender is 1.2:1:0.02:0.5. After the reaction is completed, cooling and discharging to obtain a modified polyurethane;
[0030] (4) adding nano-alumina to a mixed solvent of ethanol and deionized water, dispersing by ultrasonication, stirring evenly, and then adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:1.2, reacting at 70° C. for 10 h, centrifuging after the reaction, washing and drying to obtain amino-treated nano-alumina;
[0031] (5) adding aminated nano-alumina and p-hydroxybenzaldehyde to a reactor, reacting at 70° C. for 6 hours, and then adding diethyl phosphite, wherein the mass ratio of aminated nano-alumina, p-hydroxybenzaldehyde, and diethyl phosphite is 0.9:1:1.1, reacting at 70° C. for 6 hours, and then distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0032] (6) adding phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stirring evenly, heating in a water bath at 60° C., adding 2,3-epoxypropyltrimethylammonium chloride under constant pressure, wherein the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride is 1:1.1, reacting for 5 hours, and after the reaction, removing the solvent by reduced pressure distillation, washing and drying to obtain modified nano-alumina;
[0033] (7) Add 20 parts by weight of aqueous polyurethane dispersion, 10 parts by weight of modified polyurethane, 5 parts by weight of modified nano-alumina, 5 parts by weight of acrylic resin, 8 parts by weight of polyvinyl alcohol, and 1 part by weight of pure water into a stirrer and stir evenly at a stirring speed of 600 r / min for 10 min to obtain a water-based paint containing nanomaterials.
[0034] Example 2
[0035] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 60° C. for 4 hours, and then continuing to add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1.2:1:1.3, and continuing the reaction for 25 hours. After the reaction is completed, cooling, suction filtering and drying are performed to obtain phosphorus-containing modified thiazole;
[0036] (2) adding 2,2-bis(bromomethyl)-1,3-propanediol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propanediol to phosphorus-modified thiazole is 1:1.6, stirring evenly, and then adding 6 mol / L sodium hydroxide aqueous solution, reflux reaction at 60° C. for 18 h. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0037] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst thereto, introducing nitrogen protection, and then adding a phosphorus-containing chain extender, wherein the mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender is 1.5:1:0.04:0.9. After the reaction is completed, cooling and discharging to obtain a modified polyurethane;
[0038] (4) adding nano-alumina to a mixed solvent of ethanol and deionized water, dispersing by ultrasonication, stirring evenly, and then adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:1.4, reacting at 90° C. for 12 h, centrifuging after the reaction, washing and drying to obtain amino-treated nano-alumina;
[0039] (5) adding aminated nano-alumina and p-hydroxybenzaldehyde to a reactor, reacting at 80° C. for 8 hours, adding diethyl phosphite after the reaction, wherein the mass ratio of aminated nano-alumina, p-hydroxybenzaldehyde, and diethyl phosphite is 1.4:1:1.2, reacting at 80° C. for 10 hours, distilling under reduced pressure after the reaction, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0040] (6) adding phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stirring evenly, heating in a water bath at 80° C., adding 2,3-epoxypropyltrimethylammonium chloride under constant pressure, wherein the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride is 1:1.3, reacting for 8 hours, and after the reaction, removing the solvent by reduced pressure distillation, washing and drying to obtain modified nano-alumina;
[0041] (7) Add 30 parts by weight of aqueous polyurethane dispersion, 15 parts by weight of modified polyurethane, 8 parts by weight of modified nano-alumina, 15 parts by weight of acrylic resin, 12 parts by weight of polyvinyl alcohol, and 2 parts by weight of pure water into a stirrer and stir evenly at a stirring speed of 800 r / min for 15 min to obtain a water-based paint containing nanomaterials.
[0042] Example 3
[0043] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 50° C. for 3 hours, and then continuing to add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1.15:1:1.2, and continuing the reaction for 22.5 hours. After the reaction is completed, cooling, suction filtering and drying are performed to obtain phosphorus-containing modified thiazole;
[0044] (2) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to phosphorus-modified thiazole is 1:1.4, stirring evenly, and then adding 5 mol / L sodium hydroxide aqueous solution, reflux reaction at 50° C. for 15 h. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0045] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst thereto, introducing nitrogen protection, and then adding a phosphorus-containing chain extender, wherein the mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender is 1.35:1:0.03:0.7. After the reaction is completed, cooling and discharging to obtain a modified polyurethane;
[0046] (4) adding nano-alumina to a mixed solvent of ethanol and deionized water, dispersing by ultrasonication, stirring evenly, and then adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:1.3, reacting at 80° C. for 11 h, centrifuging after the reaction, washing and drying to obtain amino-modified nano-alumina;
[0047] (5) adding aminated nano-alumina and p-hydroxybenzaldehyde to a reactor, reacting at 75° C. for 7 hours, adding diethyl phosphite after the reaction, wherein the mass ratio of aminated nano-alumina, p-hydroxybenzaldehyde, and diethyl phosphite is 1.15:1:1.15, reacting at 75° C. for 8 hours, distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0048] (6) adding phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stirring evenly, heating in a water bath at 70° C., adding 2,3-epoxypropyltrimethylammonium chloride under constant pressure, wherein the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride is 1:1.2, reacting for 6.5 hours, and after the reaction, removing the solvent by reduced pressure distillation, washing and drying to obtain modified nano-alumina;
[0049] (7) Add 25 parts by weight of aqueous polyurethane dispersion, 12.5 parts by weight of modified polyurethane, 6.5 parts by weight of modified nano-alumina, 10 parts by weight of acrylic resin, 10 parts by weight of polyvinyl alcohol, and 1.5 parts by weight of pure water into a stirrer and stir evenly at a stirring speed of 700 r / min for 12.5 min to obtain a water-based paint containing nanomaterials.
[0050] Example 4
[0051] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 40° C. for 2 hours, and then continuing to add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1.1:1:1.1, and continuing the reaction for 20 hours. After the reaction is completed, cooling, suction filtering and drying are performed to obtain phosphorus-containing modified thiazole;
[0052] (2) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to phosphorus-modified thiazole is 1:1.2, stirring evenly, and then adding 6 mol / L sodium hydroxide aqueous solution, reflux reaction at 40° C. for 12 h. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0053] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst thereto, introducing nitrogen protection, and then adding a phosphorus-containing chain extender, wherein the mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender is 1.5:1:0.04:0.9. After the reaction is completed, cooling and discharging to obtain a modified polyurethane;
[0054] (4) adding nano-alumina to a mixed solvent of ethanol and deionized water, dispersing by ultrasonication, stirring evenly, and then adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:1.4, reacting at 90° C. for 12 h, centrifuging after the reaction, washing and drying to obtain amino-treated nano-alumina;
[0055] (5) adding aminated nano-alumina and p-hydroxybenzaldehyde to a reactor, reacting at 75° C. for 7 hours, adding diethyl phosphite after the reaction, wherein the mass ratio of aminated nano-alumina, p-hydroxybenzaldehyde, and diethyl phosphite is 1.15:1:1.15, reacting at 75° C. for 8 hours, distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0056] (6) adding phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stirring evenly, heating in a water bath at 70° C., adding 2,3-epoxypropyltrimethylammonium chloride under constant pressure, wherein the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride is 1:1.2, reacting for 6.5 hours, and after the reaction, removing the solvent by reduced pressure distillation, washing and drying to obtain modified nano-alumina;
[0057] (7) Add 25 parts by weight of aqueous polyurethane dispersion, 12.5 parts by weight of modified polyurethane, 6.5 parts by weight of modified nano-alumina, 10 parts by weight of acrylic resin, 10 parts by weight of polyvinyl alcohol, and 1.5 parts by weight of pure water into a stirrer and stir evenly at a stirring speed of 700 r / min for 12.5 min to obtain a water-based paint containing nanomaterials.
[0058] Example 5
[0059] (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 60° C. for 4 hours, and then continuing to add 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, wherein the mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1.2:1:1.3, and continuing the reaction for 25 hours. After the reaction is completed, cooling, suction filtering and drying are performed to obtain phosphorus-containing modified thiazole;
[0060] (2) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to phosphorus-modified thiazole is 1:1.6, stirring evenly, and then adding 4 mol / L sodium hydroxide aqueous solution, reflux reaction at 60° C. for 18 h. After the reaction is completed, cooling to room temperature, neutralizing, filtering, evaporating the solvent from the filtrate, washing and drying to obtain a phosphorus-containing chain extender;
[0061] (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst thereto, introducing nitrogen protection, and then adding a phosphorus-containing chain extender, wherein the mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst, and phosphorus-containing chain extender is 1.35:1:0.03:0.7. After the reaction is completed, cooling and discharging to obtain a modified polyurethane;
[0062] (4) adding nano-alumina to a mixed solvent of ethanol and deionized water, dispersing by ultrasonication, stirring evenly, and then adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:1.3, reacting at 80° C. for 11 h, centrifuging after the reaction, washing and drying to obtain amino-modified nano-alumina;
[0063] (5) adding aminated nano-alumina and p-hydroxybenzaldehyde to a reactor, reacting at 70° C. for 6 hours, and then adding diethyl phosphite, wherein the mass ratio of aminated nano-alumina, p-hydroxybenzaldehyde, and diethyl phosphite is 0.9:1:1.1, reacting at 70° C. for 6 hours, and then distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina;
[0064] (6) adding phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stirring evenly, heating in a water bath at 60° C., adding 2,3-epoxypropyltrimethylammonium chloride under constant pressure, wherein the mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride is 1:1.1, reacting for 5 hours, and after the reaction, removing the solvent by reduced pressure distillation, washing and drying to obtain modified nano-alumina;
[0065] (7) Add 20 parts by weight of aqueous polyurethane dispersion, 10 parts by weight of modified polyurethane, 5 parts by weight of modified nano-alumina, 5 parts by weight of acrylic resin, 8 parts by weight of polyvinyl alcohol, and 1 part by weight of pure water into a stirrer and stir evenly at a stirring speed of 600 r / min for 10 min to obtain a water-based paint containing nanomaterials.
[0066] Comparative Example 1
[0067] The difference between this comparative example and Example 5 is that no modified polyurethane is added.
[0068] Comparative Example 2
[0069] The difference between this comparative example and Example 5 is that no modified nano-alumina is added.
[0070] Antibacterial property: tested in accordance with the standard GB / T21866-2008 "Determination of antibacterial property and antibacterial effect of antibacterial coatings (paint films)";
[0071] Table 1: Antimicrobial testing.
[0072]
[0073] As can be seen from Table 1, the antibacterial rates of Examples 1-5 are better than those of Comparative Examples 1-2, indicating that the water-based paint containing nanomaterials prepared by the present invention has good antibacterial effect.
[0074] Use an oxygen index meter to test the limiting oxygen index of water-based paint; use a horizontal and vertical combustion instrument to test the combustion level of water-based paint.
[0075] Table 2: Flame retardancy test.
[0076] project Limiting oxygen index (%) Combustion level Example 1 29 V-0 Example 2 31 V-0 Example 3 35 V-0 Example 4 34 V-0 Example 5 31 V-0 Comparative Example 1 21 V-1 Comparative Example 2 22 V-2
[0077] It can be seen from Table 2 that the flame retardant effect of Examples 1-5 is better than that of Comparative Examples 1-2, which indicates that the water-based paint containing nanomaterials prepared by the present invention has a good flame retardant effect.
[0078] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A water-based paint containing nanomaterials, characterized in that: The invention comprises the following components by weight: 20-30 parts by weight of aqueous polyurethane dispersion, 10-15 parts by weight of modified polyurethane, 5-8 parts by weight of modified nano-alumina, 5-15 parts by weight of acrylic resin, 8-12 parts by weight of polyvinyl alcohol, and 1-2 parts by weight of pure water; The preparation method of the modified polyurethane is: (1) adding p-hydroxybenzaldehyde and 2-aminothiazole to a reactor containing an ethanol solvent, stirring evenly, introducing nitrogen protection, reacting at 40-60°C for 2-4 hours, and then adding 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and continuing the reaction for 20-25 hours. After the reaction is completed, cooling, filtering and drying are performed to obtain phosphorus-containing modified thiazole; (2) Add 2,2-bis(bromomethyl)-1,3-propanediol and phosphorus-modified thiazole to N,N-dimethylformamide solvent, stir evenly, then add 4-6 mol / L sodium hydroxide aqueous solution, reflux at 40-60°C for 12-18h. After the reaction is completed, cool to room temperature, neutralize, filter, evaporate the solvent from the filtrate, wash and dry to obtain a phosphorus-containing chain extender; (3) adding polyether polyol and hexamethylene diisocyanate into a reactor, stirring evenly, then adding dibutyltin dilaurate catalyst, introducing nitrogen protection, and then adding a phosphorus-containing chain extender. After the reaction is completed, cooling and discharging the material to obtain a modified polyurethane; The mass ratio of p-hydroxybenzaldehyde, 2-aminothiazole, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in (1) is 1.1-1.2:1:1.1-1.3; The mass ratio of 2,2-bis(bromomethyl)-1,3-propanediol to phosphorus-modified thiazole in (2) is 1:1.2-1.6; The mass ratio of polyether polyol, hexamethylene diisocyanate, dibutyltin dilaurate catalyst and phosphorus-containing chain extender in (3) is 1.2-1.5:1:0.02-0.04:0.5-0.9; The preparation method of the modified nano alumina is: S1. Add nano-alumina to a mixed solvent of ethanol and deionized water, disperse by ultrasonication, stir evenly, then continue to add γ-aminopropyltriethoxysilane, react at 70-90°C for 10-12h, centrifuge after the reaction, wash and dry to obtain amino-alumina nano-alumina; S2. Adding the amino nano-alumina and p-hydroxybenzaldehyde to the reactor, reacting at 70-80°C for 6-8h, adding diethyl phosphite, reacting at 70-80°C for 6-10h, distilling under reduced pressure, washing, and recrystallizing the crude product to obtain phosphorus-modified nano-alumina; S3. Add phosphorus-modified nano-alumina to N,N-dimethylformamide solvent, stir evenly, heat in a water bath at 60-80°C, add 2,3-epoxypropyltrimethylammonium chloride under constant pressure, react for 5-8h, remove the solvent by distillation under reduced pressure, wash and dry to obtain modified nano-alumina; The mass ratio of nano-alumina to γ-aminopropyltriethoxysilane in S1 is 1:1.2-1.4; The mass ratio of the amino nano-alumina, p-hydroxybenzaldehyde and diethyl phosphite in S2 is 0.9-1.4:1:1.1-1.2; The mass ratio of phosphorus-modified nano-alumina to 2,3-epoxypropyltrimethylammonium chloride in S3 is 1:1.1-1.
3.
2. A method for preparing a water-based paint containing nanomaterials as claimed in claim 1, characterized in that: The preparation method of the water-based paint containing nano materials comprises the following steps: adding water-based polyurethane dispersion, modified polyurethane, modified nano aluminum oxide, acrylic resin, polyvinyl alcohol and pure water into a stirrer, stirring evenly at a stirring speed of 600-800 r / min and a stirring time of 10-15 min to obtain the water-based paint containing nano materials.
Citation Information
Cited By
Modified inorganic particle doped water-based paint and preparation method thereof
CN119463601A
A modified inorganic particle doped water-based paint and preparation method thereof
CN119463601B