A method for recovering gold from gold thiosulfate by electrochemical reduction
Through the electrochemical reduction method of multi-stage pore activated carbon material electrode plates, the problem of low recovery rate of low concentration gold thiosulfate is solved, efficient recycling and simplified process flow are achieved, and large-scale production is suitable.
Patent Information
- Application Number
- CN202410402340.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-03
AI Technical Summary
The prior art cannot efficiently recover low-concentration gold thiosulfate, which has low recovery rate and complex process. It is especially suitable for high-concentration gold-immersion liquids, and the uneven pore size distribution of traditional activated carbon electrodes leads to low recovery efficiency.
Using multi-stage pore activated carbon materials as electrode plates, the efficient recovery of low-concentration gold thiosulfate is achieved through electrochemical reduction, including activated carbon materials with microporous, mesoporous and macroporous structures, which improves the specific surface area and pore volume and simplifies the process. process.
It achieves 100% recovery rate of low-concentration gold thiosulfate, is low-priced, is suitable for large-scale mass production, and simplifies the traditional process flow.
Smart Images

Figure CN118345450B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precious metal recovery, and in particular to a method for recovering gold from gold thiosulfate by electrochemical reduction. Background Art
[0002] The thiosulfate gold extraction process has the advantages of fast leaching rate, high leaching efficiency, non-toxicity and environmental friendliness at the leaching end. It is widely used to extract gold from urban mines or gold-containing ores. It is the most promising non-cyanide gold extraction method for industrial application. At present, the methods for extracting thiosulfate gold from the leachate include displacement precipitation, adsorption, solvent extraction and electrolytic deposition.
[0003] The displacement precipitation method uses a metal with stronger activity than gold as a displacement agent to replace the gold complex ions to obtain gold element, but simultaneously precipitates the divalent copper in the solution, which affects the purity of the product. In addition, when oxygen exists in the solution, the metal is easily oxidized and passivated, which affects the progress of the displacement reaction; the adsorption method is to enrich and recover the gold complex ions through physical or chemical action, but the recovery rate is extremely low, and the gold complex ions need to be eluted after enrichment, and the process flow is cumbersome; the solvent extraction method is a method of extracting from different solvents by ion exchange and chelation based on the difference in solubility of the solute in different solvents. It is suitable for high-concentration gold leaching solution, and the leaching solution needs to be clarified before extraction. The process is complicated and the cost is high, which is not suitable for industrial application; the electrolytic deposition method applies voltage to the electrolytic cell solution to generate current to achieve the purpose of depositing the desired substance on the electrode plate. The complex ions are deposited on the cathode plate in the form of a single substance, which has the advantages of small footprint and simple process, but due to the large molecular weight of the gold thiosulfate complex ions, it is difficult to migrate to the electrode interface in the solution under the electric field, so the recovery rate of low-concentration gold complex ions is low.
[0004] Therefore, it is urgent to develop a new process to achieve efficient recovery of macromolecular gold complex ions in solution. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a method for recovering gold in gold thiosulfate by electrochemical reduction, so as to solve the problem that low-concentration gold thiosulfate cannot be efficiently recovered at present.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] The present invention provides a method for recovering gold in gold thiosulfate by electrochemical reduction, comprising the following steps: placing two electrode plates provided with multi-level porous activated carbon material layers as cathodes and cathodes, respectively, in an electrolytic cell containing a gold thiosulfate solution, the multi-level porous activated carbon material layers on the two electrode plates being arranged facing each other, and connecting the two electrode plates to an external power supply to perform electrochemical reduction to recover gold in the gold thiosulfate;
[0008] Wherein, the multi-level porous activated carbon material includes micropores, mesopores and macropores.
[0009] Preferably, the concentration of the gold thiosulfate solution is a ppm level or ppb level low concentration gold thiosulfate solution.
[0010] Preferably, the gold thiosulfate solution is alkaline.
[0011] Preferably, the method for preparing the electrode plate provided with a multi-level porous activated carbon material layer comprises:
[0012] providing a substrate;
[0013] A slurry containing a multi-level porous activated carbon material is provided, and the slurry is coated on one side or both sides of the substrate, and after drying, the electrode plate provided with the multi-level porous activated carbon material layer is obtained.
[0014] Preferably, the preparation method of the multi-level porous activated carbon material is a physical or chemical activation method.
[0015] The beneficial effects of the present invention are:
[0016] The present invention adopts multi-level porous activated carbon electrode to electrochemically reduce gold thiosulfate, thereby enhancing the recovery effect of low-concentration gold thiosulfate, and the recovery rate can reach 100%. Gold is recovered in the form of single gold, simplifying the traditional process flow; the multi-level porous activated carbon material used is low in price and can be mass-produced on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a pore size distribution diagram of the activated carbon materials in Examples 1 to 4 and Comparative Example 1;
[0018] Figure 2 It is a diagram showing the recovery effect of gold in Examples 1 to 4 and Comparative Example 1. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] The electrochemical reduction method of the present invention introduces electrode materials on the basis of electrodeposition, realizes the enrichment of low-concentration gold complex ions, and realizes one-step reduction recovery. Activated carbon is a commonly used electrode material, which has the advantages of being cheap and mass-producible. However, due to the small specific surface area, uneven pore size distribution, small total pore volume, and small micropore volume of traditional activated carbon, the recovery efficiency of electrochemical reduction recovery of gold thiosulfate using traditional activated carbon as an electrode is not high and the recovery capacity is small. In order to improve the electrosorption reduction efficiency and capacity of the activated carbon electrode, the present invention also activates, modifies and expands the activated carbon, develops new pores and expansions on the basic pores, produces a developed pore structure, increases its specific surface area or pore volume, and realizes efficient recovery of gold complex ions in low-concentration leaching solution.
[0021] Specifically, the method for electrochemical reduction and recovery of gold in gold thiosulfate provided in an embodiment of the present invention comprises the following steps: two electrode plates provided with multi-level porous activated carbon material layers are respectively used as anode and cathode, and are placed in an electrolytic cell containing a gold thiosulfate solution, the multi-level porous activated carbon material layers on the two electrode plates are arranged facing each other, and the two electrode plates are connected to an external power supply to perform electrochemical reduction and recovery of gold in gold thiosulfate; wherein the multi-level porous activated carbon material comprises micropores, mesopores and macropores.
[0022] Furthermore, in some embodiments, the micropore content of the multi-level porous activated carbon material is (252-1017)×10 -3 mL / g, mesoporous content is (30~518)×10 -3 mL / g, macropore content is (3~27)×10 -3 mL / g.
[0023] Furthermore, in some embodiments, the concentration of the gold thiosulfate solution is a ppm-level or ppb-level low-concentration gold thiosulfate solution. The concentration of the gold thiosulfate solution includes but is not limited to 0.01 to 100 mg / L, and more preferably 1 to 10 mg / L; for example, it can be 0.01 mg / L, 1 mg / L, 5 mg / L, 10 mg / L, etc.
[0024] Further, in some embodiments, the gold thiosulfate solution is alkaline. In some more preferred embodiments, the pH of the gold thiosulfate solution is 8-12.
[0025] Furthermore, in some embodiments, the voltage of the electrochemical reduction is ≥0.4V, preferably 0.4-1.6V; for example, it can be 0.4V, 0.5V, 0.8V, 1.0V, 1.2V, 1.4V, 1.6V, etc.
[0026] Furthermore, in some embodiments, the spacing distance between the two electrode plates is 2-14 mm.
[0027] Furthermore, in some embodiments, the method for preparing the electrode plate provided with the multi-level porous activated carbon material layer comprises:
[0028] providing a substrate;
[0029] A slurry containing a multi-level porous activated carbon material is provided, and the slurry is coated on one side or both sides of the substrate, and after drying, the electrode plate provided with the multi-level porous activated carbon material layer is obtained.
[0030] Furthermore, in some embodiments, the substrate is a metal-based or carbon-based plate, such as a titanium plate, a platinum plate, a stainless steel plate, a nickel foam plate, or the like.
[0031] Furthermore, in some embodiments, the slurry includes a multi-level porous activated carbon material, a conductive material and a binder. The conductive material includes but is not limited to conductive carbon black, and the binder includes but is not limited to polyvinylidene fluoride.
[0032] Furthermore, in some embodiments, the preparation method of the multi-level porous activated carbon material is a physical or chemical activation method; for example, an acid or alkaline steam activation method.
[0033] Further, in some embodiments, the preparation method of the multi-level porous activated carbon material is an alkali steam activation method, specifically: the activated carbon material is mixed and ground with potassium hydroxide, calcined at high temperature, washed and dried to obtain the multi-level porous activated carbon material. The high temperature calcination temperature is 500-800°C, and the calcination time is 100-130min. As a more preferred embodiment, the high temperature calcination temperature is 700°C, and the calcination time is 120min.
[0034] The present invention is described in detail below with reference to specific embodiments.
[0035] The activated carbon materials used in the following examples are all obtained by calcining walnut shell powder at 400° C. for 60 min in a nitrogen atmosphere. In the accompanying drawings, Multi-AC represents porous activated carbon.
[0036] Example 1
[0037] A method for recovering gold from gold thiosulfate by electrochemical reduction, comprising the following steps:
[0038] (1) The activated carbon material and potassium hydroxide were ground and mixed in a mass ratio of 1:3, calcined at 500°C for 120 min under a nitrogen atmosphere, then washed with hydrochloric acid and deionized water, and freeze-dried to obtain a hierarchical activated carbon material.
[0039] (2) The multi-level porous activated carbon material is mixed with conductive carbon black and polyvinylidene fluoride (dissolved in NN dimethylacetamide) in a ratio of 8:1:1 and ground to obtain a slurry, which is evenly coated on the surface of a titanium plate, dried at 60°C for 2 hours, immersed in deionized water for 6 hours, and dried again to obtain a multi-level porous activated carbon electrode plate.
[0040] (3) Add a certain amount of ammonium thiosulfate to 190 mL of deionized water, and add 1 mL of 1000 mg / L gold standard solution (HAuCl 4 ) The pH was adjusted to maintain within the alkaline range to prevent the decomposition of thiosulfate ions, and finally the pH was adjusted to 10 and the volume was fixed to 200 mL to obtain a 5 mg / L gold thiosulfate solution.
[0041] (4) Pour the prepared gold thiosulfate solution into the electrolytic cell, place two multi-level porous activated carbon electrode plates with the coated side facing each other, immerse them in the gold thiosulfate solution with a spacing of 5 mm, start the peristaltic pump to make the solution peristaltic at a speed of 45 rpm, and connect the two electrode plates to the positive and negative poles of the power supply, respectively, and apply an external voltage of 1.2 V to recover the gold element in the gold thiosulfate.
[0042] Example 2
[0043] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the calcination temperature in step (1) is 600°C.
[0044] Example 3
[0045] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the calcination temperature in step (1) is 700°C.
[0046] Example 4
[0047] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the calcination temperature in step (1) is 800°C.
[0048] Example 5
[0049] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the concentration of the gold thiosulfate solution in step (3) is 1 mg / L.
[0050] Example 6
[0051] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the concentration of the gold thiosulfate solution in step (3) is 2 mg / L.
[0052] Example 7
[0053] The gold in the gold thiosulfate was recovered by a method substantially the same as that in Example 1, except that the concentration of the gold thiosulfate solution in step (3) was 7 mg / L.
[0054] Example 8
[0055] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the concentration of the gold thiosulfate solution in step (3) is 10 mg / L.
[0056] Example 9
[0057] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the pH of the gold thiosulfate solution in step (3) is 8.
[0058] Example 10
[0059] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the pH of the gold thiosulfate solution in step (3) is 9.
[0060] Embodiment 11
[0061] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the pH of the gold thiosulfate solution in step (3) is 11.
[0062] Example 12
[0063] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that the pH of the gold thiosulfate solution in step (3) is 12.
[0064] Embodiment 13
[0065] The gold in gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that in step (4), the spacing d between the two multi-level porous activated carbon electrode plates is 2 mm.
[0066] Embodiment 14
[0067] The gold in gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that in step (4), the spacing d between the two multi-level porous activated carbon electrode plates is 8 mm.
[0068] Embodiment 15
[0069] The gold in gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that in step (4), the spacing d between the two multi-level porous activated carbon electrode plates is 11 mm.
[0070] Example 16
[0071] The gold in gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that in step (4), the spacing d between the two multi-level porous activated carbon electrode plates is 14 mm.
[0072] Embodiment 17
[0073] The gold in the gold thiosulfate is recovered by a method substantially the same as in Example 1, except that an external voltage of 0.4 V is applied in step (4).
[0074] Embodiment 18
[0075] The gold in the gold thiosulfate is recovered by a method substantially the same as in Example 1, except that an external voltage of 0.8 V is applied in step (4).
[0076] Embodiment 19
[0077] The gold in the gold thiosulfate is recovered by a method substantially the same as in Example 1, except that an external voltage of 1.6 V is applied in step (4).
[0078] Comparative Example 1
[0079] A method for recovering gold from gold thiosulfate by electrochemical reduction, comprising the following steps:
[0080] (1) Activated carbon material, conductive carbon black and polyvinylidene fluoride (dissolved in NN-dimethylacetamide) were mixed and ground in a ratio of 8:1:1 to obtain a slurry, and the slurry was evenly coated on the surface of a titanium plate, dried at 60°C for 2 h, soaked in deionized water for 6 h, and dried again to obtain an activated carbon electrode plate.
[0081] (2) Add a certain amount of ammonium thiosulfate to 190 mL of deionized water, and add 1 mL of 1000 mg / L gold standard solution (HAuCl 4 ) The pH was adjusted to maintain within the alkaline range to prevent the decomposition of thiosulfate ions, and finally the pH was adjusted to 10 and the volume was fixed to 200 mL to obtain a 5 mg / L gold thiosulfate solution.
[0082] (3) Pour the prepared gold thiosulfate solution into the electrolytic cell, place two activated carbon electrode plates with the coated side facing each other, immerse them in the gold thiosulfate solution with a spacing of 5 mm, start the peristaltic pump to make the solution peristaltic at a speed of 45 rpm, connect the two electrode plates to the positive and negative poles of the power supply, apply an external voltage of 1.2 V, and recover the gold in the gold thiosulfate.
[0083] Comparative Example 2
[0084] The gold in the gold thiosulfate is recovered by a method substantially the same as that in Example 1, except that an external voltage of 0 V is applied in step (4).
[0085] Performance Testing
[0086] The pore size and pore volume were obtained by using a fully automatic surface area pore size analyzer, Beijing Jin Ao Pu Technology Co., Ltd., V-Sorb X800;
[0087] The recovery rate (R) and adsorption amount (Q) were calculated by the following formula:
[0088]
[0089]
[0090] Where R is the recovery rate, %; Q is the adsorption amount, mg / g; C 0 is the initial concentration of gold, mg / L; C t is the residual gold concentration at sampling time t, mg / L; V is the initial volume of the solution, L; V t is the volume of the remaining solution at sampling time t, L; m is the mass of the electrode material, mg.
[0091] (1) The pore size distribution of the activated carbon materials in Examples 1 to 4 and Comparative Example 1 was tested respectively. The results are as follows: Figure 1 And as shown in Table 1.
[0092] (2) The concentration of gold thiosulfate in the solution of Examples 1 to 4 and Comparative Example 1 after electrochemical reduction for 22 h was tested respectively, and the recovery rate and adsorption amount were calculated. The results are shown in Tables 1 and Figure 2 shown.
[0093] Table 1 Performance test results of Examples 1 to 4 and Comparative Example 1
[0094]
[0095] (3) The concentration of gold thiosulfate in the solution of Examples 5 to 19 and Comparative Example 2 after electrochemical reduction for 22 hours was tested respectively, and the recovery rate was calculated. The results are shown in Table 2.
[0096] Table 2 Performance test results of Examples 5 to 19 and Comparative Example 2
[0097]
[0098]
[0099] From Tables 1 to 2 and Figures 1-2It can be seen that the porous structure of activated carbon increases the specific surface area and can provide adsorption and reaction active sites for the reaction. Different pore structures have different effects. Micropores can greatly increase the specific surface area of the material and enhance the electrostatic interaction between the electrode material and the target ions in the solution. The present invention shows different recovery performances when used for the recovery of gold thiosulfate solution by regulating the pore size of activated carbon. In summary, the multi-level porous activated carbon electrode developed by the present invention can efficiently realize the electrochemical reduction recovery of low-concentration gold thiosulfate, and the recovery rate of low-concentration gold solution can reach 100%, which simplifies the traditional process flow.
[0100] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0101] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for recovering gold from gold thiosulfate by electrochemical reduction, It is characterized in that The steps include: Two electrode plates provided with multi-level porous activated carbon material layers are respectively used as anode and cathode, and are placed in an electrolytic cell containing a gold thiosulfate solution, the multi-level porous activated carbon material layers on the two electrode plates are arranged facing each other, and the two electrode plates are connected to an external power supply to perform electrochemical reduction to recover gold in the gold thiosulfate; Wherein, the multi-level porous activated carbon material includes micropores, mesopores and macropores.
2. The method according to claim 1, It is characterized in that The concentration of the gold thiosulfate solution is a low-concentration gold thiosulfate solution at the ppm level or ppb level.
3. The method according to claim 1, It is characterized in that The gold thiosulfate solution is alkaline.
4. The method according to claim 1, It is characterized in that The method for preparing the electrode plate provided with a multi-level porous activated carbon material layer comprises: providing a substrate; A slurry containing a multi-level porous activated carbon material is provided, and the slurry is coated on one side or both sides of the substrate, and after drying, the electrode plate provided with the multi-level porous activated carbon material layer is obtained.