Preparation and application of nano titanium dioxide with high photocatalytic activity
By using tetrabutyl titanate and modified carbon nanospheres combined with sol-gel method and solvothermal method to prepare nano titanium dioxide, and treating it with bismuth nitrate, the problem of insufficient response of nano titanium dioxide to visible light was solved and its photocatalytic activity was significantly improved. and thermal stability.
Patent Information
- Application Number
- CN202410477524.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-19
AI Technical Summary
The bandgap of nanometer titanium dioxide is wide, resulting in low response to visible light, and electrons and holes are easy to recombine, which limits the improvement of photocatalytic efficiency.
Using tetrabutyl titanate as the titanium source and modified carbon nanospheres as the dopant, the carbon nanospheres doped with titanium dioxide nanoparticles were prepared by combining the sol-gel method and the solvothermal method, and were treated with bismuth nitrate aqueous solution to form nanometer titanium dioxide with high photocatalytic activity. Titanium dioxide.
It improves the photocatalytic activity of nano-titanium dioxide, enhances the response to visible light, inhibits the recombination of electrons and holes, accelerates the photocatalytic oxidation degradation rate, and improves thermal stability and crystallinity.
Smart Images

Figure BDA0004800929960000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalysis, and in particular to the preparation and application of nano titanium dioxide with high photocatalytic activity. Background Art
[0002] Nanomaterials are an important field of current research, and the research on various preparation methods has also become a hot topic. As a semiconductor material, nano-titanium dioxide is widely used in photocatalysis, solar cells, gas sensors and other fields due to its photocatalytic activity, stable chemical properties and non-toxicity. A large number of studies have shown that nano-titanium dioxide photocatalysis can not only degrade alkanes, olefins, fatty alcohols, phenols, carboxylic acids, various simple aromatic compounds and corresponding halides, dyes, surfactants, herbicides, pesticides and other organic substances in water and air, but also can deposit inorganic metal ions such as platinum, gold, rhodium, chromium and other ions in water, and can also convert cyanide, nitrite and other ions into non-toxic forms. In addition to its application in water and air purification, research on nano-titanium dioxide in sterilization, photolysis of water, nitrogen fixation, and reduction of carbon dioxide has also made certain progress.
[0003] However, nano-titanium dioxide has some disadvantages as a photocatalyst that cannot be ignored. First, the band gap of nano-titanium dioxide is wide, which means that its response to visible light is low; second, the excited electron-holes are easy to recombine, which is a difficult problem to solve. These problems greatly limit the further improvement of the photocatalytic efficiency of nano-titanium dioxide. Therefore, it is very necessary to invent a nano-titanium dioxide with high photocatalytic activity. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation and application of nano titanium dioxide with high photocatalytic activity to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A preparation method for nano titanium dioxide with high photocatalytic activity, characterized in that the preparation method for the nano titanium dioxide with high photocatalytic activity is as follows: tetrabutyl titanate is used as a titanium source, modified carbon nanospheres are used as a doping modifier, polyethylene glycol and hexadecyltrimethylammonium bromide are used as a mixed template, an inhibitor is added, and a sol-gel method and a solvent thermal method are combined to prepare the carbon nanosphere-doped nano titanium dioxide; the carbon nanosphere-doped nano titanium dioxide is treated with a bismuth nitrate aqueous solution to prepare the nano titanium dioxide.
[0007] As an optimization, the modified carbon nanospheres are prepared by hydrothermal reaction of glucose, and the carbon nanospheres are sequentially reacted with 3-aminopropyltriethoxysilane and 2-formylthiazole to prepare the carbon nanospheres.
[0008] As an optimization, the preparation of the high photocatalytic activity nano titanium dioxide includes the following preparation steps:
[0009] (1) Mix glucose and deionized water in a mass ratio of 1:(10-12) and place them in a hydrothermal reactor for hydrothermal reaction at 180-200°C for 7-9h, cool to room temperature, centrifuge and separate, wash the precipitate with anhydrous ethanol and deionized water for 3-5 times respectively, dry at 3-5Pa and 70-80°C for 7-9h to obtain carbon nanospheres; immerse the carbon nanospheres in a silane hydrolyzate, ultrasonically treat for 1-2h, filter, and dry at 50-60°C for 7-8h to obtain pre-modified carbon nanospheres; mix the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile in a mass ratio of 1:(1.2-1.4):(8-10) and react at 70-72°C and 300-500r / min for 2-3h, filter, wash with deionized water for 3-5 times, and dry at 5-7Pa and 50-60°C for 4-6h to obtain modified carbon nanospheres;
[0010] (2) Tetrabutyl titanate, an inhibitor, and anhydrous ethanol are mixed evenly at a mass ratio of 1:(2-3):(4-6) to prepare a titanium source reaction solution; polyethylene glycol, a cationic surfactant, and an ethanol aqueous solution with a mass ratio of 0.6-0.8 times the mass of tetrabutyl titanate are mixed evenly at a mass ratio of 1:(3-4):(18-20), and then modified carbon nanospheres with a mass ratio of 0.2-0.4 times the mass of tetrabutyl titanate are added, mixed evenly, and prepared into a carbon source reaction solution; at 10-30°C, 300-5 Under stirring conditions of 00r / min, the titanium source reaction liquid is uniformly added dropwise to the carbon source reaction liquid within 5 minutes, and stirring is continued for 8-10 hours. The reaction liquid is placed in a reaction kettle and kept at 110-130°C, 140-160°C, and 170-190°C for 2-3 hours, respectively, cooled to room temperature, washed with anhydrous ethanol and deionized water for 3-5 times respectively, dried at 3-5Pa, 50-60°C for 5-6 hours, and ground into a powder with a particle size of 8-10nm to obtain carbon nanospheres doped with nano-titanium dioxide;
[0011] (3) bismuth nitrate and a nitric acid aqueous solution with a mass fraction of 1 to 2% are mixed uniformly in a mass ratio of 1:(20 to 30) to prepare a bismuth nitrate aqueous solution; carbon nanospheres doped with nano-titanium dioxide in an amount 3 to 4 times the mass of bismuth nitrate are added to the bismuth nitrate aqueous solution, stirred at 70 to 80° C. and 300 to 500 r / min for 3 to 4 hours, dried at 3 to 5 Pa and 50 to 60° C. for 5 to 6 hours, placed in a muffle furnace, and calcined at 350 to 370° C. for 3 to 4 hours to obtain nano-titanium dioxide with high photocatalytic activity.
[0012] As an optimization, the silane hydrolyzate in step (1) is prepared by uniformly mixing 3-aminopropyltriethoxysilane, anhydrous ethanol and deionized water in a mass ratio of 1:(2.2-2.5):(8-10), and adjusting the pH to 4.8-5.0 with a hydrochloric acid aqueous solution with a mass fraction of 10-12%.
[0013] As an optimization, the inhibitor in step (2) is glacial acetic acid.
[0014] As an optimization, the model of the polyethylene glycol in step (2) is PEG4000.
[0015] As an optimization, the cationic surfactant in step (2) is hexadecyltrimethylammonium bromide.
[0016] As an optimization, the mass fraction of the ethanol aqueous solution in step (2) is 30-40%.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0018] When preparing nano titanium dioxide with high photocatalytic activity, the present invention prepares carbon nanospheres by hydrothermal reaction of glucose; the carbon nanospheres are sequentially reacted with 3-aminopropyltriethoxysilane and 2-formylthiazole to prepare modified carbon nanospheres; tetrabutyl titanate is used as a titanium source, glacial acetic acid is used as an inhibitor, polyethylene glycol and hexadecyltrimethylammonium bromide are used as a mixed template, and the modified carbon nanospheres are used as a doping modifier, and a sol-gel method and a solvent thermal method are combined to prepare carbon nanosphere doped nano titanium dioxide; the carbon nanosphere doped nano titanium dioxide is treated with a bismuth nitrate aqueous solution to prepare nano titanium dioxide with high photocatalytic activity.
[0019] Firstly, glucose is subjected to a hydrothermal reaction to obtain carbon nanospheres; the carbon nanospheres are sequentially reacted with 3-aminopropyltriethoxysilane and 2-formylthiazole to obtain modified carbon nanospheres; the carbon material has a strong response to visible light, which makes up for the wide bandgap of titanium dioxide material and weak response to visible light; when visible light is irradiated on the composite material, the electrons in the carbon nanospheres are transferred from the carbon material to the conduction band of titanium dioxide, providing more substances participating in the reaction for the photocatalytic process, thereby improving the photocatalytic activity of nano titanium dioxide with high photocatalytic activity; the surface of the carbon nanospheres is rich in a large number of hydroxyl groups, the carbon nanospheres are reacted with 3-aminopropyltriethoxysilane to introduce amino groups on the surface of the carbon nanospheres, and then reacted with 2-formylthiazole to form a carbon nanosphere on the surface of the carbon nanospheres. A thiazole Schiff base structure is generated. When the carbon nanospheres doped with nano-titanium dioxide are treated with an aqueous bismuth nitrate solution, the thiazole Schiff base structure can form a metal coordination bond with metal bismuth, and bismuth is modified on the surface and pores of the nano-titanium dioxide with high photocatalytic activity. Bismuth can inhibit the aggregation of anatase phase grains and inhibit phase change, thereby improving the thermal stability and crystallinity of the nano-titanium dioxide with high photocatalytic activity, forming bismuth trioxide-titanium dioxide composite nanoparticles, improving the separation efficiency of photogenerated carriers, and further improving the response of the nano-titanium dioxide with high photocatalytic activity in the visible light region, effectively inhibiting the recombination of electrons and holes, increasing the speed of electron transfer to oxygen, accelerating the rate of photocatalytic oxidation degradation, and further improving the photocatalytic activity of the nano-titanium dioxide with high photocatalytic activity.
[0020] Secondly, tetrabutyl titanate was used as a titanium source, glacial acetic acid was used as an inhibitor, polyethylene glycol and hexadecyltrimethylammonium bromide were used as a mixed template, and modified carbon nanospheres were used as doping modifiers. The carbon nanospheres doped with nano-titanium dioxide were prepared by combining the sol-gel method and the solvothermal method. The carbon nanospheres doped with nano-titanium dioxide were treated with a bismuth nitrate aqueous solution to obtain nano-titanium dioxide with high photocatalytic activity. During the reaction, glacial acetic acid formed a chelate with titanium, which inhibited the hydrolysis and polycondensation of tetrabutyl titanate, making the crystallization process of titanium dioxide easier to control. Polyethylene glycol and cationic The surfactant hexadecyltrimethylammonium bromide is used as a mixed template, and the particles are surrounded by surfactant molecules, and the environment for coagulation or growth between particles is destroyed, making the formed nano titanium dioxide particles smaller; polyethylene glycol can also combine with titanium to hinder the further growth of grains and reduce the particle size of high photocatalytic activity nano titanium dioxide. After high-temperature calcination, polyethylene glycol will decompose to produce gas and form a porous structure, which increases the specific surface area of high photocatalytic activity nano titanium dioxide and further improves the photocatalytic activity of high photocatalytic activity nano titanium dioxide. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] A method for preparing nano titanium dioxide with high photocatalytic activity, the method comprising the following steps:
[0024] (1) Glucose and deionized water were mixed in a mass ratio of 1:10, placed in a hydrothermal reactor, hydrothermally reacted at 180°C for 9 hours, cooled to room temperature, centrifuged, and the precipitate was washed with anhydrous ethanol and deionized water for 3 times each, and dried at 3Pa, 70°C for 9 hours to obtain carbon nanospheres; 3-aminopropyltriethoxysilane, anhydrous ethanol, and deionized water were mixed in a mass ratio of 1:2.2:8, and dissolved in 10% hydrochloric acid. The pH of the solution was adjusted to 4.8 to obtain a silane hydrolyzate; the carbon nanospheres were immersed in the silane hydrolyzate, ultrasonically treated for 1 hour, filtered, and dried at 50°C for 8 hours to obtain pre-modified carbon nanospheres; the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile were mixed uniformly in a mass ratio of 1:1.2:8, stirred at 70°C and 300 r / min for 3 hours, filtered, washed with deionized water for 3 times, and dried at 5Pa and 50°C for 6 hours to obtain modified carbon nanospheres;
[0025] (2) Tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol are mixed in a mass ratio of 1:2:4 to prepare a titanium source reaction solution; polyethylene glycol, hexadecyltrimethylammonium bromide, and an ethanol aqueous solution with a mass fraction of 30% are mixed in a mass ratio of 1:3:18 with a mass ratio of 0.6 times the mass of tetrabutyl titanate, and then modified carbon nanospheres with a mass fraction of 0.2 times the mass of tetrabutyl titanate are added and mixed to prepare a carbon source reaction solution; under the stirring conditions of 10°C and 300r / min, the titanium source reaction solution is uniformly added dropwise to the carbon source reaction solution within 5 minutes, and stirring is continued for 10 hours. The reaction solution is placed in a reactor and kept at 110°C, 140°C, and 170°C for 3 hours, respectively, cooled to room temperature, washed with anhydrous ethanol and deionized water for 3 times each, dried at 3Pa and 50°C for 6 hours, and ground into a powder with a particle size of 8nm to obtain carbon nanospheres doped with nano-titanium dioxide;
[0026] (3) Bismuth nitrate and a 1% nitric acid aqueous solution were mixed in a mass ratio of 1:20 to prepare a bismuth nitrate aqueous solution; carbon nanospheres doped with nano-titanium dioxide in an amount three times the mass of bismuth nitrate were added to the bismuth nitrate aqueous solution, stirred at 70°C and 300 r / min for 4 h, dried at 3Pa and 50°C for 6 h, placed in a muffle furnace, and calcined at 350°C for 4 h to obtain nano-titanium dioxide with high photocatalytic activity.
[0027] Example 2
[0028] A method for preparing nano titanium dioxide with high photocatalytic activity, the method comprising the following steps:
[0029] (1) Glucose and deionized water were mixed in a mass ratio of 1:11, placed in a hydrothermal reactor, hydrothermally reacted at 190°C for 8 hours, cooled to room temperature, centrifuged, and the precipitate was washed 4 times with anhydrous ethanol and deionized water, respectively, and dried at 4Pa, 75°C for 8 hours to obtain carbon nanospheres; 3-aminopropyltriethoxysilane, anhydrous ethanol, and deionized water were mixed in a mass ratio of 1:2.35:9, and adjusted with a hydrochloric acid aqueous solution with a mass fraction of 11%. pH to 4.9, to obtain a silane hydrolyzate; immerse the carbon nanospheres in the silane hydrolyzate, ultrasonically treat for 1.5 hours, filter, and dry at 55°C for 7.5 hours to obtain pre-modified carbon nanospheres; mix the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile in a mass ratio of 1:1.3:9, stir and react at 71°C, 400r / min for 2.5 hours, filter, wash with deionized water 4 times, and dry at 6Pa, 55°C for 5 hours to obtain modified carbon nanospheres;
[0030] (2) Tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol were mixed in a mass ratio of 1:2.5:5 to prepare a titanium source reaction solution; polyethylene glycol (0.7 times the mass of tetrabutyl titanate), hexadecyltrimethylammonium bromide, and 35% ethanol aqueous solution (mass fraction) were mixed in a mass ratio of 1:3.5:19, and then modified carbon nanospheres (0.3 times the mass of tetrabutyl titanate) were added and mixed to prepare a carbon source reaction solution; under stirring conditions of 20°C and 400 r / min, the titanium source reaction solution was uniformly added dropwise to the carbon source reaction solution within 5 minutes, and stirring was continued for 9 hours. The mixture was placed in a reactor and kept at 120°C, 150°C, and 180°C for 2.5 hours, cooled to room temperature, washed with anhydrous ethanol and deionized water 4 times each, dried at 4Pa and 55°C for 5.5 hours, and ground into a powder with a particle size of 9 nm to obtain carbon nanospheres doped with nano-titanium dioxide;
[0031] (3) Bismuth nitrate and a 1.5% nitric acid aqueous solution were mixed uniformly at a mass ratio of 1:25 to prepare a bismuth nitrate aqueous solution; carbon nanospheres doped with nano-titanium dioxide in an amount 3.5 times the mass of bismuth nitrate were added to the bismuth nitrate aqueous solution, stirred at 75°C and 400 r / min for 3.5 h, dried at 4Pa and 55°C for 5.5 h, placed in a muffle furnace, and calcined at 360°C for 3.5 h to obtain nano-titanium dioxide with high photocatalytic activity.
[0032] Example 3
[0033] A method for preparing nano titanium dioxide with high photocatalytic activity, the method comprising the following steps:
[0034] (1) Glucose and deionized water were mixed in a mass ratio of 1:12, placed in a hydrothermal reactor, hydrothermally reacted at 200°C for 7 hours, cooled to room temperature, centrifuged, and the precipitate was washed 5 times with anhydrous ethanol and deionized water, respectively, and dried at 5Pa, 80°C for 7 hours to obtain carbon nanospheres; 3-aminopropyltriethoxysilane, anhydrous ethanol, and deionized water were mixed in a mass ratio of 1:2.5:10, and dissolved in 12% hydrochloric acid. The pH of the solution was adjusted to 5.0 to obtain a silane hydrolyzate; the carbon nanospheres were immersed in the silane hydrolyzate, ultrasonically treated for 2 hours, filtered, and dried at 60°C for 7 hours to obtain pre-modified carbon nanospheres; the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile were mixed uniformly at a mass ratio of 1:1.4:10, stirred at 72°C and 500r / min for 2 hours, filtered, washed with deionized water for 5 times, and dried at 7Pa and 60°C for 4 hours to obtain modified carbon nanospheres;
[0035] (2) Tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol are mixed in a mass ratio of 1:3:6 to prepare a titanium source reaction solution; polyethylene glycol, hexadecyltrimethylammonium bromide, and an ethanol aqueous solution with a mass fraction of 40% are mixed in a mass ratio of 1:4:20 with a mass ratio of 0.8 times the mass of tetrabutyl titanate, and then modified carbon nanospheres with a mass fraction of 0.4 times the mass of tetrabutyl titanate are added and mixed to prepare a carbon source reaction solution; under stirring conditions of 30°C and 500 r / min, the titanium source reaction solution is uniformly added dropwise to the carbon source reaction solution within 5 minutes, and stirring is continued for 8 hours. The reaction solution is placed in a reactor and kept at 130°C, 160°C, and 190°C for 2 hours, respectively, cooled to room temperature, washed with anhydrous ethanol and deionized water for 5 times each, dried at 5Pa and 60°C for 5 hours, and ground into a powder with a particle size of 10 nm to obtain carbon nanospheres doped with nano-titanium dioxide;
[0036] (3) Bismuth nitrate and a 2% nitric acid aqueous solution were mixed uniformly at a mass ratio of 1:30 to prepare a bismuth nitrate aqueous solution; carbon nanospheres doped with nano-titanium dioxide in an amount 4 times the mass of bismuth nitrate were added to the bismuth nitrate aqueous solution, stirred at 80°C and 500 r / min for 3 h, dried at 5Pa and 60°C for 5 h, placed in a muffle furnace, and calcined at 370°C for 3 h to obtain nano-titanium dioxide with high photocatalytic activity.
[0037] Comparative Example 1
[0038] The preparation of high photocatalytic activity nano titanium dioxide in Comparative Example 1 is different from that in Example 2 in that step (1) is not performed, and step (2) is modified as follows: tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol are mixed uniformly in a mass ratio of 1:2.5:5 to prepare a titanium source reaction solution; polyethylene glycol with a mass ratio of 0.7 times that of tetrabutyl titanate, hexadecyltrimethylammonium bromide, and an ethanol aqueous solution with a mass fraction of 35% are mixed uniformly in a mass ratio of 1:3.5:19 to prepare a template reaction solution; under stirring conditions of 20°C and 400r / min, the titanium source reaction solution is uniformly added dropwise to the template reaction solution within 5min, and stirring is continued for 9h, and the reaction is placed in a reactor and heated at 120°C, 400r / min, 500r / min, 1000r / min, 2000r / min, 3000r / min, 4000r / min, 5000r / min, 2000r / min, 3000r / min, 4 ... Keep warm at 150℃ and 180℃ for 2.5h, cool to room temperature, wash with anhydrous ethanol and deionized water 4 times each, dry at 4Pa, 55℃ for 5.5h, grind into powder with a particle size of 9nm, and prepare nano titanium dioxide; modify step (3) as follows: mix bismuth nitrate and 1.5% nitric acid aqueous solution in a mass ratio of 1:25 to prepare a bismuth nitrate aqueous solution; add 3.5 times the mass of bismuth nitrate nano titanium dioxide to the bismuth nitrate aqueous solution, stir at 75℃, 400r / min for 3.5h, dry at 4Pa, 55℃ for 5.5h, place in a muffle furnace, and roast at 360℃ for 3.5h to prepare nano titanium dioxide with high photocatalytic activity. The remaining steps are the same as those in Example 2.
[0039] Comparative Example 2
[0040] The preparation of high photocatalytic activity nano titanium dioxide in Comparative Example 2 is different from that in Example 2 in step (1), where step (1) is modified as follows: glucose and deionized water are mixed evenly in a mass ratio of 1:11, placed in a hydrothermal reactor, subjected to hydrothermal reaction at 190° C. for 8 h, cooled to room temperature, centrifuged, and the precipitate is washed 4 times with anhydrous ethanol and deionized water, respectively, and dried at 4 Pa, 75° C. for 8 h to obtain modified carbon nanospheres. The remaining steps are the same as in Example 2.
[0041] Comparative Example 3
[0042] The preparation of high photocatalytic activity nano titanium dioxide in comparative example 3 is different from that in example 2 only in step (2), and step (2) is modified as follows: tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol are mixed at a mass ratio of 1:2.5:5 to prepare a titanium source reaction solution; modified carbon nanospheres 0.3 times the mass of tetrabutyl titanate and an ethanol aqueous solution with a mass fraction of 35% are mixed at a mass ratio of 1:19 to prepare a carbon source reaction solution; under stirring conditions of 20°C and 400r / min, the titanium source reaction solution is uniformly added dropwise to the carbon source reaction solution within 5min, and stirring is continued for 9h, and the reaction solution is placed in a reactor, and kept at 120°C, 150°C, and 180°C for 2.5h, cooled to room temperature, washed with anhydrous ethanol and deionized water 4 times each, dried at 4Pa, 55°C for 5.5h, and ground into a powder with a particle size of 9nm to prepare carbon nanosphere-doped nano titanium dioxide. The remaining steps are the same as in example 2.
[0043] Comparative Example 4
[0044] The preparation of high photocatalytic activity nano titanium dioxide in Comparative Example 4 is different from that in Example 2 in that step (3) is not performed, and step (2) is modified as follows: tetrabutyl titanate, glacial acetic acid, and anhydrous ethanol are mixed uniformly in a mass ratio of 1:2.5:5 to prepare a titanium source reaction solution; polyethylene glycol, hexadecyltrimethylammonium bromide, and an ethanol aqueous solution with a mass fraction of 35% are mixed uniformly in a mass ratio of 1:3.5:19 with a mass ratio of 0.7 times the mass of tetrabutyl titanate, and then 0.3 times the mass of tetrabutyl titanate are added. The modified carbon nanospheres were mixed evenly to prepare a carbon source reaction solution; under the stirring conditions of 20°C and 400r / min, the titanium source reaction solution was uniformly added to the carbon source reaction solution within 5 minutes, and the stirring was continued for 9 hours. The mixture was placed in a reactor and kept at 120°C, 150°C, and 180°C for 2.5 hours, cooled to room temperature, washed with anhydrous ethanol and deionized water 4 times each, dried at 4Pa and 55°C for 5.5 hours, and ground into a powder with a particle size of 9nm to obtain nano titanium dioxide with high photocatalytic activity. The remaining steps were the same as in Example 2.
[0045] Test Example 1
[0046] Photocatalytic activity test
[0047] Test method: This experiment uses a 300W xenon lamp to simulate visible light (λ>420nm), degrades methyl orange under its irradiation, and tests the absorbance of the solution after illumination to characterize the photocatalytic ability of high photocatalytic activity nano titanium dioxide; the specific steps are: weigh 50mg of the embodiment and the comparative example and disperse them in 50mL of a 10mg / L methyl orange aqueous solution, stir continuously and uniformly for 30min under completely light-proof conditions to achieve adsorption-desorption equilibrium, place 14cm below the xenon lamp, turn on the xenon lamp, sample 4ml each time at a set time interval, centrifuge the mixed solution after the reflection, take the upper liquid after centrifugation and test the absorbance of the solution to be tested in a UV-visible spectrophotometer model UV1901PC produced by Shanghai Youke Co., Ltd. The maximum absorption wavelength of methyl orange is 464nm, which is used as the test basis, and the relative concentration of the solution is calculated according to the standard curve of methyl orange, and the apparent rate constant is fitted to characterize the photocatalytic rate of the sample. The results are shown in Table 1.
[0048] Table 1
[0049]
[0050] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the high photocatalytic activity nano titanium dioxide prepared in the present invention has good photocatalytic performance.
[0051] By comparison, the apparent rate constants of Examples 1 to 3 are greater than those of Comparative Examples 1, 2, and 4, indicating that glucose is reacted to obtain carbon nanospheres through a hydrothermal reaction; carbon nanospheres are reacted with 3-aminopropyltriethoxysilane and 2-formylthiazole in sequence to obtain modified carbon nanospheres; carbon materials have a strong response to visible light, which makes up for the wide bandgap of titanium dioxide materials and weak response to visible light. When visible light is irradiated on the composite material, electrons in the carbon nanospheres are transferred from the carbon material to the conduction band of titanium dioxide, providing more substances participating in the reaction for the photocatalytic process, thereby improving the photocatalytic activity of nano titanium dioxide with high photocatalytic activity; the surface of the carbon nanospheres is rich in a large number of hydroxyl groups, and the carbon nanospheres are reacted with 3-aminopropyltriethoxysilane to introduce amino groups on the surface of the carbon nanospheres, and then The thiazole Schiff base structure is generated on the surface of the carbon nanospheres by reacting with 2-formyl thiazole. When the carbon nanospheres doped with nano-titanium dioxide are treated with an aqueous bismuth nitrate solution, the thiazole Schiff base structure can form a metal coordination bond with metal bismuth, thereby modifying bismuth on the surface and in the pores of the nano-titanium dioxide with high photocatalytic activity. Bismuth can inhibit the aggregation of anatase phase grains and inhibit phase change, thereby improving the thermal stability and crystallinity of the nano-titanium dioxide with high photocatalytic activity, forming bismuth trioxide-titanium dioxide composite nanoparticles, improving the separation efficiency of photogenerated carriers, and further improving the response of the nano-titanium dioxide with high photocatalytic activity in the visible light region, effectively inhibiting the recombination of electrons and holes, increasing the speed of electron transfer to oxygen, accelerating the rate of photocatalytic oxidation degradation, and further improving the photocatalytic activity of the nano-titanium dioxide with high photocatalytic activity.
[0052] By comparison, the apparent rate constants of Examples 1 to 3 are greater than that of Comparative Example 3, indicating that carbon nanospheres doped with nano-titanium dioxide are prepared by combining sol-gel method and solvent thermal method with tetrabutyl titanate as titanium source, glacial acetic acid as inhibitor, polyethylene glycol and hexadecyltrimethylammonium bromide as mixed templates, and modified carbon nanospheres as doping modifiers; the carbon nanospheres doped with nano-titanium dioxide are treated with bismuth nitrate aqueous solution to prepare nano-titanium dioxide with high photocatalytic activity; polyethylene glycol and cationic surfactant hexadecyltrimethylammonium bromide are used as mixed templates, the particles are surrounded by surfactant molecules, the environment for coagulation or growth between particles is destroyed, and the formed nano-titanium dioxide particles are smaller; polyethylene glycol can also combine with titanium to hinder the further growth of grains and reduce the particle size of nano-titanium dioxide with high photocatalytic activity. Polyethylene glycol will decompose and produce gas after high-temperature calcination to form a porous structure, increase the specific surface area of nano-titanium dioxide with high photocatalytic activity, and further improve the photocatalytic activity of nano-titanium dioxide with high photocatalytic activity.
[0053] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing nano titanium dioxide with high photocatalytic activity, It is characterized in that The method for preparing the nano titanium dioxide with high photocatalytic activity is to treat the carbon nanospheres doped with nano titanium dioxide with a bismuth nitrate aqueous solution; The preparation method of carbon nanosphere doped nano titanium dioxide comprises: uniformly mixing tetrabutyl titanate, an inhibitor and anhydrous ethanol at a mass ratio of 1:(2-3):(4-6) to prepare a titanium source reaction solution; uniformly mixing polyethylene glycol with a mass ratio of 0.6-0.8 times the mass of tetrabutyl titanate, a cationic surfactant and an ethanol aqueous solution with a mass ratio of 1:(3-4):(18-20), and then adding modified carbon nanospheres with a mass ratio of 0.2-0.4 times the mass of tetrabutyl titanate, mixing uniformly to prepare a carbon source reaction solution; and heating for 10-20 minutes. Under stirring conditions of 30°C and 300-500r / min, the titanium source reaction liquid was uniformly added dropwise to the carbon source reaction liquid within 5 minutes, and stirring was continued for 8-10 hours. The mixture was placed in a reactor and kept at 110-130°C, 140-160°C, and 170-190°C for 2-3 hours, cooled to room temperature, washed with anhydrous ethanol and deionized water for 3-5 times each, dried at 3-5Pa and 50-60°C for 5-6 hours, and ground into a powder with a particle size of 8-10 nm to obtain carbon nanospheres doped with nano-titanium dioxide; The preparation method of the modified carbon nanospheres is as follows: glucose and deionized water are mixed uniformly at a mass ratio of 1:(10-12), placed in a hydrothermal reactor, hydrothermally reacted at 180-200° C. for 7-9 hours, cooled to room temperature, centrifuged, and the precipitate is washed with anhydrous ethanol and deionized water for 3-5 times respectively, and dried at 3-5 Pa and 70-80° C. for 7-9 hours to obtain carbon nanospheres; the carbon nanospheres are immersed in a silane hydrolyzate and ultrasonically treated for 1 ~2h, filtered, and dried at 50~60℃ for 7~8h to obtain pre-modified carbon nanospheres; the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile are evenly mixed in a mass ratio of 1:(1.2~1.4):(8~10), stirred at 70~72℃, 300~500r / min for 2~3h, filtered, washed with deionized water for 3~5 times, and dried at 5~7Pa, 50~60℃ for 4~6h to obtain modified carbon nanospheres.
2. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 1, It is characterized in that The modified carbon nanospheres are prepared by hydrothermal reaction of glucose, and then reacting the carbon nanospheres with 3-aminopropyltriethoxysilane and 2-formylthiazole in sequence.
3. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 1, It is characterized in that The method comprises the following preparation steps: (1) Glucose and deionized water were mixed evenly at a mass ratio of 1:(10-12), placed in a hydrothermal reactor, and subjected to hydrothermal reaction at 180-200°C for 7-9 hours. The mixture was cooled to room temperature and centrifuged. The precipitate was washed with anhydrous ethanol and deionized water for 3-5 times each, and dried at 3-5 Pa and 70-80°C for 7-9 hours to obtain carbon nanospheres. The carbon nanospheres were immersed in a silane hydrolyzate, subjected to ultrasonic treatment for 1-2 hours, and filtered. , dried at 50-60°C for 7-8h to obtain pre-modified carbon nanospheres; the pre-modified carbon nanospheres, 2-formyl thiazole, and acetonitrile were mixed uniformly in a mass ratio of 1:(1.2-1.4):(8-10), stirred at 70-72°C, 300-500r / min for 2-3h, filtered, washed with deionized water for 3-5 times, and dried at 5-7Pa, 50-60°C for 4-6h to obtain modified carbon nanospheres; (2) Tetrabutyl titanate, inhibitor, and anhydrous ethanol are mixed evenly in a mass ratio of 1:(2-3):(4-6) to prepare a titanium source reaction solution; polyethylene glycol (0.6-0.8 times the mass of tetrabutyl titanate), a cationic surfactant, and an ethanol aqueous solution are mixed evenly in a mass ratio of 1:(3-4):(18-20), and then modified carbon nanospheres (0.2-0.4 times the mass of tetrabutyl titanate) are added and mixed evenly to prepare a carbon source reaction solution; the mixture is heated at 10-30°C and 300-5 Under stirring conditions of 00r / min, the titanium source reaction liquid was uniformly added dropwise to the carbon source reaction liquid within 5 minutes, and stirring was continued for 8-10 hours. The reaction liquid was placed in a reactor and kept at 110-130°C, 140-160°C, and 170-190°C for 2-3 hours, respectively, cooled to room temperature, washed with anhydrous ethanol and deionized water for 3-5 times each, dried at 3-5Pa, 50-60°C for 5-6 hours, and ground into a powder with a particle size of 8-10nm to obtain carbon nanospheres doped with nano-titanium dioxide; (3) Bismuth nitrate and 1-2% nitric acid aqueous solution were mixed in a mass ratio of 1:(20-30) to prepare a bismuth nitrate aqueous solution; carbon nanospheres doped with nano-titanium dioxide in an amount 3-4 times the mass of bismuth nitrate were added to the bismuth nitrate aqueous solution, stirred at 70-80°C and 300-500 r / min for 3-4 h, dried at 3-5 Pa and 50-60°C for 5-6 h, placed in a muffle furnace, and calcined at 350-370°C for 3-4 h to obtain nano-titanium dioxide with high photocatalytic activity.
4. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 3, It is characterized in that The silane hydrolyzate in step (1) is prepared by uniformly mixing 3-aminopropyltriethoxysilane, anhydrous ethanol and deionized water in a mass ratio of 1:(2.2-2.5):(8-10), and adjusting the pH to 4.8-5.0 with a 10-12% mass fraction hydrochloric acid aqueous solution.
5. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 3, It is characterized in that The inhibitor in step (2) is glacial acetic acid.
6. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 3, It is characterized in that The model of the polyethylene glycol in step (2) is PEG4000.
7. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 3, It is characterized in that The cationic surfactant in step (2) is hexadecyltrimethylammonium bromide.
8. A method for preparing nano titanium dioxide with high photocatalytic activity according to claim 3, It is characterized in that The mass fraction of the ethanol aqueous solution in step (2) is 30-40%.
9. Use of nano titanium dioxide with high photocatalytic activity prepared according to any one of claims 1 to 8 in photocatalytic degradation of methyl orange.
Citation Information
Patent Citations
Method for preparing bismuth-doped nano-titanium dioxide photocatalyst