Lipophilic carbon-phosphorus composite sodium negative electrode material and preparation method thereof
Using pumpkin peel as a precursor, the lipophilic carbon-phosphorus composite sodium electronegative electrode material is prepared, which solves the cycle life problem of sodium-ion batteries, improves the cycle stability and first charge and discharge efficiency of the battery, and realizes an environmentally friendly and low-cost preparation method.
Patent Information
- Application Number
- CN202410788230.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Sodium-ion batteries cause the negative electrode carbon material skeleton to collapse during charge and discharge cycles, which affects the cycle life of the battery. It is difficult to achieve high first charge and discharge efficiency and improve cycle performance with existing technology.
Pumpkin peels are used as biomass precursors, and lipophilic carbon-phosphorus composite sodium electrode materials are prepared through steps such as carbonization, hydrothermal reaction, ball milling and pickling. The carbonization temperature, introduction of organic functional groups and inorganic doping are controlled to form excellent electrode materials. chemical properties.
It improves the cycle stability of sodium-ion batteries, realizes a simple, safe and environmentally friendly preparation method, reduces costs, and promotes the recycling of waste materials, which has environmental significance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium battery negative electrode materials, and in particular relates to an oleophilic carbon-phosphorus composite sodium battery negative electrode material and a preparation method thereof. Background Art
[0002] With the continuous development of new energy technology, sodium-ion batteries have attracted much attention. With the continuous development of sodium-ion battery technology and the reduction of costs, commercial applications and research are becoming more and more extensive.
[0003] Chinese invention patent publication number CN115020654A proposes a method for preparing a hard carbon composite material for sodium ion batteries. After grinding porous carbon and black phosphorus, add them to a metal compound catalyst solution, filter them, and deposit a carbon source on their surface by chemical vapor deposition to obtain a hard carbon precursor material; the obtained hard carbon precursor is pressed into a sheet structure and pressed together with a sodium sheet, and an electrolyte is added, placed in a microwave oven, and pre-sodiumized to obtain a hard carbon composite material. Black phosphorus has a layered structure similar to graphite, with a large interlayer spacing, which is suitable for the storage of sodium ions. Chinese invention patent publication number CN115528232A discloses a method for preparing a reed-derived hard carbon sodium negative electrode material and an energy storage battery. The preparation of the reed-derived hard carbon negative electrode material is achieved by the phosphoric acid pyrolysis method. When phosphoric acid is heated to 500-600°C, it decomposes to produce oxides, such as P4O 10 Or P2O5, by adding phosphorus element, the thermal stability of the battery will be further improved.
[0004] Sodium ions will cause the collapse of the negative electrode carbon material skeleton during the charge and discharge cycle, thus affecting the cycle life of the battery. Hard carbon is the most valuable negative electrode material for sodium ion batteries. In order to achieve large-scale commercial application of sodium ion batteries, it is necessary to find suitable precursors and preparation methods to achieve higher initial charge and discharge efficiency and further improve the cycle performance. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a lipophilic carbon-phosphorus composite sodium negative electrode material, which selects low-priced and abundant biomass as a precursor, and obtains a sodium ion battery negative electrode material with excellent electrochemical performance by accurately controlling the preparation conditions such as carbonization temperature, introduction of organic functional groups, and doping of inorganic substances, and is used to prepare sodium ion batteries, effectively improving the cycle stability of the battery. The preparation method of the present invention is simple, safe, environmentally friendly, and low-cost.
[0006] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material of the present invention comprises the following steps:
[0007] (1) soaking the pumpkin skin in a sodium carbonate solution to soften the pumpkin skin, and drying it in a naturally ventilated state to obtain a dried pumpkin skin;
[0008] (2) placing the dried pumpkin peel into a muffle furnace for carbonization to obtain a hard carbon material;
[0009] (3) adding the hard carbon material into a hydrothermal kettle containing a sodium dodecylbenzene sulfonate solution and heating it, and then drying it to obtain a hydrothermal reaction material;
[0010] (4) ball milling the material after the hydrothermal reaction and red phosphorus to obtain a mixed material;
[0011] (5) placing the mixed material into a tube furnace, heating it under a nitrogen atmosphere, and cooling it naturally after heating is completed;
[0012] (6) The material obtained in step (5) is placed in oxalic acid for pickling to obtain the product.
[0013] Preferably, the pumpkin peel is taken from Cucurbita cucurbita.
[0014] In step (1), the drying temperature is 27-30° C., the drying time is 24-36 h, the concentration of the sodium carbonate solution is 0.5-1.5 mol / L, and the soaking time is 6-10 h.
[0015] In step (2), during carbonization, the temperature is raised from room temperature to the carbonization temperature at a heating rate of 5-10°C / min, the carbonization temperature is 400-600°C, and the insulation time at the carbonization temperature is 2-4h.
[0016] In step (3), the concentration of the sodium dodecylbenzene sulfonate solution is 10wt.%-15wt.%, and the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is (15-20):1. During heating, the temperature is increased from room temperature to the heating temperature at a heating rate of 1-3°C / min, the heating temperature is 300-450°C, and the insulation time at the heating temperature is 2-4h; the drying temperature is 90-100°C, and the drying time is 8-10h.
[0017] In step (4), the mass ratio of the material and red phosphorus after the hydrothermal reaction is (5-8):1.
[0018] In step (4), a planetary ball mill is used for ball milling, the ball mill speed is 250-300 rpm, the ball milling time is 1-3 h, and the ball-to-material mass ratio is (7-9):1.
[0019] In step (5), the temperature is raised from room temperature to a heating temperature of 450°C-600°C at a heating rate of 1-3°C / min, and the holding time at the heating temperature is 3-5h.
[0020] In step (6), the oxalic acid concentration for pickling is 2-5 mol / L.
[0021] The lipophilic carbon-phosphorus composite sodium negative electrode material of the present invention is prepared by the above-mentioned preparation method.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The pumpkin peel used in the present invention has a relatively loose pore structure, which is conducive to drying, and the distance between layers is large, which is conducive to the embedding and extraction of sodium ions in the later stage; pumpkin peel is widely available, cheap, and is generally discarded as waste. The present invention realizes the recycling of waste materials, which has positive environmental significance;
[0024] 2. The present invention uses pumpkin peel as a carbon source for hard carbon, and introduces relevant lipophilic groups at the same time, and uses vapor deposition method to immerse red phosphorus into the hard carbon interlayer under nitrogen atmosphere to prepare an amorphous hard carbon negative electrode material;
[0025] 3. The preparation method of the present invention is simple, safe, environmentally friendly, and low-cost, which helps to improve the cycle stability and provides the possibility for further preparing sodium ion batteries with long cycle life. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0027] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0028] The pumpkin skins in Examples 1-6 and Comparative Examples 1-5 were taken from honey pumpkin.
[0029] Example 1
[0030] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0031] (1) Soaking the pumpkin peel in a 1.5 mol / L sodium carbonate solution for 8 h to soften the pumpkin peel, and air-drying the pumpkin peel at 27°C under natural ventilation for 36 h to obtain the dried pumpkin peel;
[0032] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 7°C / min, the carbonization temperature is 400°C, and the holding time at the carbonization temperature is 2 h to obtain a hard carbon material;
[0033] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 10 wt.% and heating the material from room temperature to a heating temperature of 450°C at a heating rate of 1°C / min, keeping the material at the heating temperature for 4 hours, and then drying the material at 90°C for 10 hours to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 15:1;
[0034] (4) placing the hydrothermal reaction material and red phosphorus in a planetary ball mill at a mass ratio of 5:1 for ball milling to obtain a mixed material; the ball mill speed is 280 rpm, the ball milling time is 1 h, and the ball-to-material mass ratio is 8:1;
[0035] (5) Place the mixed material in a tubular furnace and heat it in a nitrogen atmosphere from room temperature to a heating temperature of 600°C at a heating rate of 3°C / min. Keep the temperature at the heating temperature for 5 h and cool it naturally after heating.
[0036] (6) The material obtained in step (5) is placed in 3 mol / L oxalic acid for pickling.
[0037] Example 2
[0038] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0039] (1) Soaking the pumpkin peel in a 0.5 mol / L sodium carbonate solution for 6 h to soften the pumpkin peel, and drying it in air at 30° C. under natural ventilation for 24 h to obtain the dried pumpkin peel;
[0040] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 5°C / min, the carbonization temperature is 600°C, and the holding time at the carbonization temperature is 2 h to obtain a hard carbon material;
[0041] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 15 wt.% and heating the material from room temperature to a heating temperature of 400°C at a heating rate of 2°C / min, keeping the temperature at the heating temperature for 3 h, and then drying the material at 100°C for 8 h to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 20:1;
[0042] (4) The material after the hydrothermal reaction and red phosphorus were placed in a planetary ball mill at a mass ratio of 6:1 for ball milling to obtain a mixed material; the ball mill speed was 250 rpm, the ball milling time was 3 h, and the ball-to-material mass ratio was 7:1;
[0043] (5) The mixed material was placed in a tubular furnace and heated under a nitrogen atmosphere at a heating rate of 3°C / min from room temperature to a heating temperature of 450°C. The temperature was kept at the heating temperature for 5 h and then cooled naturally after the heating was completed.
[0044] (6) The material obtained in step (5) is placed in oxalic acid with a concentration of 5 mol / L for pickling.
[0045] Example 3
[0046] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0047] (1) Soaking the pumpkin peel in a 1 mol / L sodium carbonate solution for 10 h to soften the pumpkin peel, and air-drying the pumpkin peel at 28° C. under natural ventilation for 30 h to obtain the dried pumpkin peel;
[0048] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 10°C / min, the carbonization temperature is 550°C, and the holding time at the carbonization temperature is 3 h to obtain a hard carbon material;
[0049] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 12 wt.% and heating the material from room temperature to a heating temperature of 350°C at a heating rate of 3°C / min, keeping the material at the heating temperature for 2 h, and then drying the material at 90°C for 9 h to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 18:1;
[0050] (4) placing the material after the hydrothermal reaction and red phosphorus in a planetary ball mill at a mass ratio of 8:1 for ball milling to obtain a mixed material; the ball mill speed is 250 rpm, the ball milling time is 3 h, and the ball-to-material mass ratio is 9:1;
[0051] (5) The mixed material was placed in a tubular furnace and heated under a nitrogen atmosphere at a heating rate of 2°C / min from room temperature to a heating temperature of 550°C. The heating time was 4 h and the mixture was cooled naturally after the heating was completed.
[0052] (6) The material obtained in step (5) is placed in 4 mol / L oxalic acid for pickling.
[0053] Example 4
[0054] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0055] (1) Soaking the pumpkin peel in a 1.5 mol / L sodium carbonate solution for 10 h to soften the pumpkin peel, and air-drying it at 30° C. under natural ventilation for 24 h to obtain the dried pumpkin peel;
[0056] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 10°C / min, the carbonization temperature is 400°C, and the holding time at the carbonization temperature is 4 h to obtain a hard carbon material;
[0057] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 10 wt.% and heating the material from room temperature to a heating temperature of 300°C at a heating rate of 3°C / min, keeping the material at the heating temperature for 2 h, and then drying the material at 90°C for 10 h to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 20:1;
[0058] (4) placing the material after the hydrothermal reaction and red phosphorus in a planetary ball mill at a mass ratio of 6:1 for ball milling to obtain a mixed material; the ball mill speed is 300 rpm, the ball milling time is 2 h, and the ball-to-material mass ratio is 8:1;
[0059] (5) The mixed material was placed in a tubular furnace and heated under a nitrogen atmosphere at a heating rate of 1°C / min from room temperature to a heating temperature of 550°C. The holding time at the heating temperature was 4 h. After the heating was completed, the mixture was cooled naturally.
[0060] (6) The material obtained in step (5) is placed in 2 mol / L oxalic acid for pickling.
[0061] Example 5
[0062] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0063] (1) Soaking the pumpkin peel in a 1 mol / L sodium carbonate solution for 8 h to soften the pumpkin peel, and air-drying the pumpkin peel at 28° C. under natural ventilation for 24 h to obtain the dried pumpkin peel;
[0064] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 5°C / min, the carbonization temperature is 400°C, and the holding time at the carbonization temperature is 3 h to obtain a hard carbon material;
[0065] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 15 wt.% and heating the material from room temperature to a heating temperature of 400°C at a heating rate of 2°C / min, keeping the material at the heating temperature for 3 h, and then drying the material at 95°C for 8 h to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 18:1;
[0066] (4) placing the hydrothermal reaction material and red phosphorus in a planetary ball mill at a mass ratio of 7:1 for ball milling to obtain a mixed material; the ball mill speed is 280 rpm, the ball milling time is 2 h, and the ball-to-material mass ratio is 7:1;
[0067] (5) Place the mixed material in a tubular furnace and heat it in a nitrogen atmosphere from room temperature to a heating temperature of 600°C at a heating rate of 2°C / min. Keep the temperature at the heating temperature for 3 h and cool it naturally after heating is completed.
[0068] (6) The material obtained in step (5) is placed in 4 mol / L oxalic acid for pickling.
[0069] Example 6
[0070] The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material comprises the following steps:
[0071] (1) Soaking the pumpkin peel in a 0.5 mol / L sodium carbonate solution for 8 h to soften the pumpkin peel, and air-drying it at 27°C under natural ventilation for 24 h to obtain the dried pumpkin peel;
[0072] (2) placing the dried pumpkin peel in a muffle furnace for carbonization, heating the temperature from room temperature to the carbonization temperature at a heating rate of 5°C / min, the carbonization temperature is 400°C, and the holding time at the carbonization temperature is 4 h to obtain a hard carbon material;
[0073] (3) adding the hard carbon material into a hydrothermal autoclave containing a sodium dodecylbenzene sulfonate solution with a concentration of 15 wt.% and heating the material from room temperature to a heating temperature of 450°C at a heating rate of 2°C / min, keeping the temperature at the heating temperature for 3 h, and then drying the material at 90°C for 9 h to obtain the material after the hydrothermal reaction; wherein the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is 15:1;
[0074] (4) placing the material after the hydrothermal reaction and red phosphorus in a planetary ball mill at a mass ratio of 5:1 for ball milling to obtain a mixed material; the ball mill speed is 300 rpm, the ball milling time is 2 h, and the ball-to-material mass ratio is 9:1;
[0075] (5) Place the mixed material in a tubular furnace and heat it in a nitrogen atmosphere from room temperature to a heating temperature of 600°C at a heating rate of 2°C / min. Keep the temperature at the heating temperature for 4 hours and cool it naturally after heating is completed.
[0076] (6) The material obtained in step (5) is placed in 3 mol / L oxalic acid for pickling.
[0077] Comparative Example 1
[0078] The difference between this comparative example and Example 1 is that no sodium carbonate solution is used for soaking in step (1).
[0079] Comparative Example 2
[0080] The difference between this comparative example and Example 2 is that no red phosphorus is added in step (4), and the material after the hydrothermal reaction is only placed in a planetary ball mill for ball milling.
[0081] Comparative Example 3
[0082] The difference between this comparative example and Example 3 is that in step (5), no nitrogen is introduced, but the heating and compounding is carried out directly in air.
[0083] Comparative Example 4
[0084] The difference between this comparative example and Example 4 is that the ball milling speed is reduced in step (4) to 150 rpm and the ball milling time is 0.5 h.
[0085] Comparative Example 5
[0086] The difference between this comparative example and Example 5 is that in step (3), no sodium dodecylbenzene sulfonate solution is added, and deionized water is used as the hydrothermal solvent.
[0087] Comparative Example 6
[0088] The only difference between this comparative example and Example 6 is that there are no steps (1) and (2), and the hard carbon material in step (3) is conventional hard carbon (Xi'an Shaanmei Jingjiu New Energy Technology Co., Ltd., biomass hard carbon HC-300).
[0089] The materials prepared in Examples 1-6 and Comparative Examples 1-6 are used to assemble a full battery. The specific battery assembly process is as follows:
[0090] Sodium nickel iron manganese oxide was used as the positive electrode, and the prepared sodium negative electrode material was used as the negative electrode. 95mm×80mm pole pieces were prepared respectively. 1MNaPF6 was used as the electrolyte, and the organic solvent was EC:DMC:DEC=1:1:1 in volume ratio. The soft-pack sodium ion battery was assembled, and the charge and discharge test was performed at a current of 0.5C. The discharge capacity and capacity retention rate after 20 cycles of charge and discharge are shown in Table 1.
[0091] Table 1 Discharge capacity and capacity retention rate of full batteries of Examples 1-6 and Comparative Examples 1-6 after 20 cycles
[0092]
[0093] It can be seen from Table 1 that the discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 1 after 20 cycles are lower than those of the full battery assembled with the negative electrode material of Example 1. This is because the pumpkin skin is more loose after being soaked in sodium carbonate solution, and the heat is more uniform during carbonization, and the carbonization is more complete, which in turn affects the formation of the carbon skeleton, which is conducive to the discharge capacity, thereby improving the cycle stability of the battery.
[0094] The discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 2 after 20 cycles are lower than those of the full battery assembled with the negative electrode material of Example 2. This is because the addition of red phosphorus forms a POC covalent bond between carbon and phosphorus, which is not only beneficial to maintaining the stability of the SEI film, but also beneficial to maintaining the integrity of the skeleton when the hard carbon volume expands, thereby improving the Na + The deintercalation rate is beneficial to the discharge capacity, thereby improving the cycle stability of the battery.
[0095] The discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 3 after 20 cycles are lower than those of the full battery assembled with the negative electrode material of Example 3. This is because the introduction of nitrogen makes the red phosphorus dispersed in the interlayer of the nitrogen-carbon sheet. The high conductivity of the nitrogen-carbon sheet is conducive to improving the utilization rate of red phosphorus, thereby improving the specific energy of the electrode sheet, and nitrogen-carbon can form a covalent bond to improve the mechanical strength of the hard carbon, which is conducive to improving the cycle stability.
[0096] The discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 4 after 20 cycles are lower than those of the full battery assembled with the negative electrode material of Example 4. This is because the reduction of ball milling speed and ball milling time leads to excessive size of the active material, which prolongs the ion diffusion path, increases the possibility of particle pulverization during charge and discharge, reduces the electrode reaction kinetics, and affects the battery cycle stability.
[0097] The discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 5 after 20 cycles are lower than those of the full battery assembled with the negative electrode material of Example 5. - The introduction of groups makes the material lipophilic and hydrophobic, which repels H2O molecules in chemical reactions and improves its contact with organic electrolytes, which is beneficial to cycle stability.
[0098] The discharge capacity and capacity retention rate of the full battery assembled with the negative electrode material of Comparative Example 6 after 20 cycles are slightly lower than those of the full battery assembled with the negative electrode material of Example 6. This is because the pumpkin peel used as a carbon source in the present invention is easier to obtain, and the pore structure of the pumpkin peel is relatively loose, which is conducive to the drying and ball milling process, and the interlayer structure distance is relatively large, which is conducive to the embedding and extraction of sodium ions in the electrochemical reaction, and improves the cycle stability to a certain extent. The present invention also realizes waste utilization, is more environmentally friendly, and has greater environmental value.
Claims
1. A method for preparing an oleophilic carbon-phosphorus composite sodium negative electrode material, characterized in that: The following steps are involved: (1) soaking pumpkin peel in a sodium carbonate solution and drying it to obtain dried pumpkin peel; (2) carbonizing the dried pumpkin peel to obtain a hard carbon material; (3) adding the hard carbon material into a hydrothermal kettle containing a sodium dodecylbenzene sulfonate solution and heating it, and then drying it to obtain a hydrothermal reaction material; (4) ball milling the material after the hydrothermal reaction and red phosphorus to obtain a mixed material; (5) placing the mixed material into a tube furnace, heating it under a nitrogen atmosphere, and cooling it naturally after heating is completed; (6) The material obtained in step (5) is placed in oxalic acid for pickling to obtain; In step (1), the concentration of the sodium carbonate solution is 0.5-1.5 mol / L, and the soaking time is 6-10 h; In step (2), the carbonization temperature is 400-600°C, and the holding time at the carbonization temperature is 2-4h; In step (3), the concentration of the sodium dodecylbenzene sulfonate solution is 10wt.%-15wt.%, the mass ratio of the sodium dodecylbenzene sulfonate solution to the hard carbon material is (15-20):1, the heating temperature is 300-450°C, and the insulation time at the heating temperature is 2-4h; In step (4), the mass ratio of the material after the hydrothermal reaction to red phosphorus is (5-8):1, and ball milling is performed using a planetary ball mill with a ball mill speed of 250-300 rpm and a ball milling time of 1-3 h; In step (5), the heating temperature is 450°C-600°C, and the insulation time at the heating temperature is 3-5h.
2. The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material according to claim 1, characterized in that: In step (2), during carbonization, the temperature is raised from room temperature to the carbonization temperature at a heating rate of 5-10°C / min.
3. The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material according to claim 1, characterized in that: In step (3), the heating is performed at a heating rate of 1-3°C / min from room temperature to the heating temperature; the drying temperature is 90-100°C, and the drying time is 8-10h.
4. The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material according to claim 1, characterized in that: In step (4), the mass ratio of ball to material is (7-9):
1.
5. The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material according to claim 1, characterized in that: In step (5), the temperature is raised from room temperature to the heating temperature at a heating rate of 1-3°C / min.
6. The method for preparing the lipophilic carbon-phosphorus composite sodium negative electrode material according to claim 1, characterized in that: In step (6), the oxalic acid concentration for pickling is 2-5 mol / L.
7. A lipophilic carbon-phosphorus composite sodium negative electrode material, characterized in that: The method is prepared by any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of hard carbon composite material for sodium ion battery
CN115020654A
Reed-derived hard carbon sodium battery negative electrode material, preparation method thereof and energy storage battery
CN115528232A
Preparation method and application for nitrogen phosphorus co-doped porous carbon
CN107425204A
Nitrogen / phosphorus doped carbon composite catalyst as well as preparation method and application thereof
CN114142051A
Black phosphorus-carbon nanotube composite synthesized using surfactant and method of manufacturing the same and lithium secondary battery including the same
KR1020220132947A