10.9 grade hot rolled carbon reduced annealed cold heading steel wire rod and its manufacturing method

Through the chemical composition of C-Si-Mn carbon and high-temperature spinning, online salt bath weak isothermal and roller rapid cooling technology, tempered pearlite and tempered Widmansite structures are formed, solving the problem of 10.9 grade hot-rolled carbon cold heading The problem of high strength and low cracking risk of steel wire rod enables efficient manufacturing of grade 10.9 fasteners, reducing the annealing process and improving production efficiency.

CN118360552BActive Publication Date: 2024-10-01JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410797872.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The existing grade 10.9 hot-rolled carbon cold-headed steel wire rod is difficult to meet the demand for high-strength fastener manufacturing. In particular, there are challenges in reducing the spheroidizing annealing process and reducing the risk of cracking, and the high carbon content of carbon steel causes thermal The sensitivity increases and the difficulty of tissue control increases.

Method used

Designed with C-Si-Mn carbon chemical composition, through high-temperature spinning and online salt bath weak isothermal treatment, the microstructure of tempered pearlite and tempered Widmansite is formed. Combined with roller rapid cooling technology, the wire rod is controlled The plasticity and strength are improved, reducing the difficulty of annealing and improving production efficiency.

Benefits of technology

It has achieved a tensile strength of 880~910MPa and an area shrinkage rate of 57%~61%, which reduces the risk of cold working cracking, simplifies the manufacturing process, reduces the annealing process, and has good market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118360552B_ABST
    Figure CN118360552B_ABST
Patent Text Reader

Abstract

The invention relates to a 10.9-grade hot-rolled carbon reduced annealed cold heading steel wire rod and a manufacturing method thereof. The wire rod is spun at a spinning temperature of ≥960°C based on a carbon steel composition with medium C, low Si and high Mn. The wire rod is cooled to a molten salt temperature at a cooling rate of ≥36°C / s through an online salt bath weak isotherm, so that high-temperature austenite in the wire rod structure is transformed into pearlite with fine lamellar spacing and a small amount of widmanstattenite. At the same time, the wire rod is isothermally tempered to be transformed into tempered pearlite and tempered widmanstattenite, and pearlite lamellae are melted to form lamellar melted pearlite. Finally, the cold heading steel wire rod is rapidly cooled through a roller to obtain a mixed structure of mainly tempered pearlite, a small amount of tempered widmanstattenite and lamellar melted pearlite. The cold heading steel wire rod can be efficiently produced, has a tensile strength of 880-910MPa, and a cross-sectional shrinkage of 57%-61%. The wire rod is used in the application fields of manufacturing 10.9-grade high-strength fasteners, bolts, etc., and can reduce at least one annealing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled carbon wire rods, and in particular relates to a 10.9-grade hot-rolled carbon reduced annealed cold heading steel wire rod and a manufacturing method thereof. Background Art

[0002] As the structure of fastener products continues to upgrade to high-strength, the proportion of medium- and high-strength fasteners continues to increase. The production of 10.9-grade fasteners requires the cold-heading steel wire rod to be subjected to multiple drawing, multiple spheroidizing annealing, cold-heading forming and quenching and tempering treatments to meet the performance grade requirements. The spheroidizing annealing adopts the method of heating the hot-rolled wire rod after coiling or drawing to austenitization, and then annealing to spheroidize the carbides in the steel to reduce the material hardness and improve the cold deformability. However, multiple spheroidizing annealing also brings about the problems of many processes, high emissions and energy consumption. The existing hot-rolled wire rods for 10.9-grade fastener products are mainly achieved by adding elements that improve the hardenability of the material to achieve the high-strength upgrade goal of the fastener products. The carbon steel that omits the alloying elements has the advantages of low material cost and simple smelting. Therefore, it is necessary to develop 10.9-grade hot-rolled carbon-reduced annealed cold-heading steel wire rods to reduce at least one subsequent spheroidizing annealing process to meet the market demand for green manufacturing of high-strength fastener bolts.

[0003] The technical difficulties and causes of hot-rolled carbon cold-headed steel wire rod being difficult to meet the requirements of 10.9 grade fasteners reduced annealing manufacturing are as follows:

[0004] (1) The existing 10.9 grade hot-rolled cold heading steel wire rod is mainly manufactured by reducing the carbon content that affects the plastic toughness of the wire rod, adding Ti, Al, B, Mo and other material hardenability elements to ensure the strength grade, and combining the controlled cooling method of the Stelmor air cooling line. However, the addition of hardenability elements is prone to the appearance of martensite, bainite and other deteriorated plastic structures in the controlled cooling process of the Stelmor air cooling line, resulting in an increased risk of cracking during the cold working process. In order to achieve the application of reduced annealing or no annealing, low-temperature wire drawing and slow cooling are used after rolling to increase the proportion of ferrite in the structure for plasticity. Adjustment, for example: Patent CN117265408A discloses an annealing-free cold heading steel and its manufacturing method and the fastener obtained therefrom, which adopts C-Si-Mn-Al-Cr-Mo-B-Mg composition design, combined with ≤800℃ low-temperature spinning and heat preservation cooling process, to obtain ferrite + degenerate pearlite structure, reaching Rm≤650MPa, Z≥53%; but on the one hand, after omitting the hardenability element, in order to ensure the final performance level, the carbon content of carbon steel is higher than that of alloy steel, which brings about the increase of thermal sensitivity of steel. The problem is that even if the insulation cover of the Stelmore air-cooling line is closed, the wire rod is not completely transformed into austenite structure of ferrite or pearlite during the continuous cooling process. At a cooling rate of 2~5℃ / s, bainite hard-brittle phase structure will still appear at around 500℃, resulting in a significant decrease in the plasticity of the wire rod; on the other hand, after eliminating elements such as Ti, Nb, and V that inhibit the coarsening of austenite structure, carbon steel tends to coarsen at the corresponding heating temperature. With the increase of the air-cooling cooling rate, it is more likely to precipitate along the saturated solid solution crystal plane and distribute in flake or needle shape. The Widmanstatten structure has high hardness but poor plasticity and toughness, which is difficult to eliminate during the continuous controlled cooling process. Its organizational inheritance is accompanied by coarse grains, which increases the risk of cold working cracking. At the same time, the maximum cooling rate and total length of the Stelmor air cooling line are limited. By reducing the cooling rate and keeping warm to extend the online time of the wire rod to reduce the Widmanstatten abnormality, the soft phase ferrite and pearlite structure obtained will lead to too low production efficiency and final strength of the cold heading steel wire rod, increasing the demand for drawing to reduce surface and increase strength. The plasticity loss in the process is large, which is not conducive to reducing the spheroidizing annealing process.

[0005] (2) In order to reduce the spheroidizing annealing time of carbon cold heading steel, some existing technologies use low-temperature rolling to increase the distortion energy inside the steel, taking advantage of the metastable state of cementite lamellae in pearlite. After the steel is off the production line, annealing is performed to cause the cementite to melt and precipitate to rapidly spheroidize. For example, patent CN116426818A discloses a rapidly spheroidizing medium carbon steel bar and its manufacturing method, which adopts a C-Si-Mn-Cr-Al-Ca composition design, combined with low-temperature heating and ultra-low-temperature rolling to achieve a tensile strength of 545~582MPa after short-time spheroidization. However, the strength and plasticity are relatively insufficient, which easily leads to an increased risk of cracking of the hot-rolled wire rod during the drawing and cold heading process of 10.9 grade fasteners. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 10.9-grade hot-rolled carbon-reduced annealed cold-heading steel wire rod and a manufacturing method thereof. The invention designs efficient production and regulates the microstructure and performance of the hot-rolled wire rod based on the C-Si-Mn carbon chemical composition, especially improves the plasticity of the cold-heading steel wire rod, reduces the risk of cracking caused by abnormal microstructure during cold working, and is used to achieve green manufacturing of 10.9-grade high-strength fasteners by reducing at least one annealing process to meet market demand.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] A 10.9 grade hot-rolled carbon-reduced annealed cold-heading steel wire rod, the chemical composition and mass percentage of the cold-heading steel wire rod include: C: 0.42%-0.48%, Si: 0.1%-0.25%, Mn: 0.6%-0.9%, P≤0.020%, S≤0.020%, and the rest are Fe and unavoidable impurities; its microstructure includes a mixed structure composed of 70%-76% by volume of tempered pearlite, a small amount of tempered widmanstattenite and lamellar fused pearlite.

[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0010] (1) Carbon: Carbon is the most basic, effective and economical strengthening element in steel. It mainly exists in the form of cementite in cold heading steel. As the carbon content increases, the tensile strength of the steel can be significantly improved, but it will increase the cold brittleness and thermal sensitivity of the steel, reduce the proeutectoid structure, and is not conducive to the regulation of the Widmanstatten structure. Therefore, in order to reduce material costs and precipitate a small amount of Widmanstatten structure during phase transformation, without adding Ti, Al, B, Mo and other material hardenability elements, Nb, V and other elements and other grain refining elements, in order to ensure the final strength level of 10.9 grade non-adjustable fasteners, the carbon content is appropriately increased, and the mass percentage of C is controlled to be 0.42%~0.48%.

[0011] (2) Silicon: The Si element is a good deoxidizer. It can improve the hardenability and tensile strength of steel, reduce the critical cooling rate of steel, and easily promote the formation of pearlite in the structure. However, excessive silicon will increase the tendency of surface decarburization, increase the degree of cold working hardening of steel, and reduce the cold plastic deformation and toughness of steel. In order to take into account the cold heading performance of steel, the Si content is appropriately reduced. Therefore, the mass percentage of Si is controlled to be 0.1%~0.25%.

[0012] (3) Manganese: Mn is a good deoxidizer and desulfurizer. It can also improve the strength level and hardenability of wire rod through solid solution strengthening, increase the supercooling degree of austenite during cooling, and is beneficial to the refinement of pearlite and the promotion of Widmanstätten structure formation. However, too high Mn content will aggravate the segregation of steel, increase the overheating sensitivity and temper brittleness tendency of steel, and have an adverse effect on the plasticity and structure control of steel. In order to take into account the strength, structure control and cold working performance of steel, the Mn content is appropriately increased. Therefore, the mass percentage of Mn is controlled to be 0.6%~0.9%.

[0013] (4) Phosphorus and sulfur: Phosphorus and sulfur are impurity elements. Their concentration at grain boundaries will reduce the toughness of steel. The lower the better. Therefore, P ≤ 0.020% and S ≤ 0.020%.

[0014] Based on the above-mentioned cold heading steel wire rod adopting medium C-low Si-high Mn, omitting hardenability elements and carbon steel composition, the tempered pearlite in the microstructure retains the characteristics of moderate strength and plasticity of pearlite with higher strength than ferrite and higher plasticity than bainite. Tempering is used to further reduce the stress of pearlite structure and improve its toughness. At the same time, pearlite with fine lamellar spacing is melted to form lamellar melting pearlite to achieve the effect of comprehensively improving the plasticity of cold heading steel. The tempered widmanstatten uses the characteristics of carbon steel that austenite grains are coarser after eliminating grain refinement elements, and it is easier to precipitate widmanstatten structure due to shear mechanism and high temperature carbon diffusion transfer conditions after cooling, retaining the high hardness of widmanstatten structure, and tempering is used to significantly reduce the dislocation density of widmanstatten structure to improve plasticity and toughness, and obtain both strong and tough organizational properties. Compared with the existing method of adding After the hardenability element, the grain is refined to improve the strength of the wire rod. The above-mentioned cold heading steel wire rod is mainly tempered pearlite and a small amount of tempered widmanstattenite to provide matrix strength, which makes up for the strength loss of the band after omitting the hardenability element. Compared with the existing method of improving the plasticity of the wire rod by increasing the proportion of ferrite in the organization or simplifying annealing by using the metastable state of pearlite lamellae, the above-mentioned cold heading steel wire rod uses the tempered state of pearlite and widmanstatten structure to improve and eliminate internal stress, improve organizational stability, and significantly improve brittleness. Combined with a small amount of lamellar melt pearlite, high-plasticity cold heading steel wire rod can be obtained while taking into account the strength of the wire rod. The difficulty of annealing is reduced by reducing the dislocation density of the organization and making the lamellar melt pearlite easier to spheroidize. When used for the subsequent manufacture of 10.9 grade fasteners, at least one spheroidizing annealing process is reduced, and it has good market application prospects.

[0015] Preferably, the finer the lamellar spacing of the tempered pearlite, the higher the strength and lower the plasticity of the cold heading steel wire rod. Therefore, the lamellar spacing of the tempered pearlite can be further controlled to be 75-100 nm to regulate the strength and plasticity of the cold heading steel wire rod.

[0016] Preferably, the higher the proportion of the tempered widmanstatten body, the higher the strength of the cold heading steel wire rod and the lower the plasticity. Therefore, the volume percentage of the tempered widmanstatten body can be further controlled to be 22%~28% to regulate the strength and plasticity of the cold heading steel wire rod.

[0017] Preferably, the diameter of the cold heading steel wire rod is 6.5~18.0mm, the tensile strength is 880~910MPa, and the cross-sectional reduction rate is 57%~61%. It has high strength characteristics that are no less than those of alloyed steels. At the same time, it has significantly improved plasticity characteristics compared to the air-cooled wire rod with ferrite + pearlite structure, which is manifested as a higher cross-sectional reduction rate. Therefore, it can be used in the manufacture of 10.9 grade high-strength fasteners and bolts and other application fields, reducing at least one spheroidizing annealing process.

[0018] A method for manufacturing a 10.9 grade hot-rolled carbon-reduced annealed cold-headed steel wire rod, the manufacturing method comprising:

[0019] The wire rod is produced based on the chemical composition of the above-mentioned 10.9 grade hot-rolled carbon reduced annealed cold heading steel wire rod, the wire rod is spun into a wire rod at a spinning temperature of ≥960°C, the wire rod is subjected to weak isothermal treatment in an online salt bath, the wire rod is cooled to the molten salt temperature at a cooling rate of ≥36°C / s, the high-temperature austenite in the wire rod structure is transformed into pearlite with fine lamellar spacing and a small amount of widmanstattenite, and isothermally tempered to be transformed into tempered pearlite and tempered widmanstattenite, and the pearlite lamellar melting is promoted to form lamellar melting pearlite, and finally it is rapidly cooled by a roller to produce a cold heading steel wire rod having a microstructure including a mixed structure consisting of 70% to 76% by volume of tempered pearlite, a small amount of tempered widmanstattenite and lamellar melting pearlite.

[0020] The above manufacturing method adopts C-Si-Mn composition, and at a higher spinning temperature, the austenite grains are appropriately coarsened, and a higher proportion of widmanstattenite structure is more easily obtained. The wire rod after high-temperature spinning is directly subjected to online salt bath weak isothermal treatment through molten salt. Compared with the existing Stelmor air cooling line, the wire rod can quickly pass through the ferrite phase transformation temperature range at a higher cooling rate and a larger degree of supercooling. Compared with the strong isothermal treatment with a lower temperature and a longer time, on the basis of carbon steel composition, the online salt bath weak isothermal can avoid the precipitation of bainite or martensite structure, so that most of the high-temperature austenite in the wire rod structure after spinning is transformed into pearlite with fine lamellar spacing, and a small part of the high-temperature austenite is transformed into pearlite with fine lamellar spacing. Under the conditions of high-temperature carbon diffusion and transfer, austenite forms needle-shaped widmanstattenite structure to provide matrix strength. At the same time, compared with the existing insulation cooling or delayed cooling process, the high heat exchange capacity of molten salt is used to maintain the high-temperature isothermal state of the wire rod for a longer time, so that the pearlite is tempered to form tempered pearlite. At the same time, the pearlite with fine lamellar spacing is easily melted to form lamellar pearlite, and the dislocation density of the widmanstattenite structure is reduced to form tempered widmanstattenite. Compared with the two-stage salt bath treatment process using low temperature and high temperature respectively, the one-stage treatment method of online salt bath weak isothermal treatment makes it easier to control the molten salt temperature and it is also easy to maintain the state of the fine lamellar spacing of tempered pearlite to avoid excessive tempering softening.

[0021] After weak isothermal treatment in the online salt bath, the austenite structure in the wire rod is fully transformed, which also avoids the situation in which the carbon steel increases its sensitivity due to the increase in carbon content and precipitates hard and brittle phases during the roller rapid cooling process, affecting the uniformity of the structure. After the roller rapid cooling, it quickly reaches the coiling position, which can effectively reduce the online time and improve the production efficiency of the cold heading steel wire rod compared to the roller slow cooling process. At the same time, the roller rapid cooling can quickly cool the wire rod to prevent the wire rod from being over-tempered and softened, thereby reducing the strength grade of the wire rod. Finally, the structure, strength and plasticity of the carbon cold heading steel wire rod are matched, which is more beneficial to simplifying the manufacturing process and reducing the production cost.

[0022] Preferably, since the abnormal structures of widmanstatten and bainite are improved by online salt bath weak isothermal treatment after spinning, and a longer isothermal treatment time can be obtained compared with insulation cooling, there is no need to consider the problem of increased wear of the rolling line caused by low-temperature rolling to increase the proportion of ferrite. Therefore, the wire is produced by hot rolling, and the final rolling temperature is controlled to be 980~1010℃, the final rolling reduction is 26%~36%, and the wire grain size is ≤8 levels. On the one hand, a higher final rolling temperature can be used to reduce the wear on the rolling line and improve the rolling efficiency. On the other hand, a higher final rolling temperature and a large final rolling reduction can be used to appropriately coarsen the wire grains, so as to prepare the organization for obtaining an appropriate proportion of pearlite and widmanstatten after spinning.

[0023] Preferably, the higher the spinning temperature is, the higher the proportion of tempered widosteatite in the tissue is, and conversely, the lower the spinning temperature is, the higher the proportion of tempered pearlite in the tissue is. Therefore, the spinning temperature of the wire rod can be further controlled to control the matrix strength, and the spinning temperature is preferably ≤980°C.

[0024] Preferably, since the carbon cold heading steel wire rod is manufactured for the purpose of efficient production of cold heading steel wire rod and 10.9 grade fastener annealing reduction production, the lower the isothermal temperature and the shorter the isothermal treatment time, the finer the lamellar spacing of the tempered pearlite, so that the strength of the cold heading steel wire rod increases and the plasticity decreases. However, if the isothermal temperature is too low, bainite or even martensite will appear, causing a significant loss of strength. If the isothermal treatment time is too short, the pearlite and widmanstattenite are not completely tempered, causing the brittleness of the cold heading steel wire rod to increase significantly. Conversely, the higher the isothermal temperature and the longer the isothermal treatment time, the coarser the lamellar spacing of the tempered pearlite. As the isothermal treatment time increases, the energy storage of the lamellar pearlite increases, and the proportion of lamellar melted pearlite increases, which reduces the strength of the cold heading steel wire rod and increases the plasticity. However, if the isothermal temperature is too high, the spacing between the pearlite lamellae will be large, which will lead to a large spacing between the lamellae of the tempered pearlite, and is not conducive to melting to form lamellar pearlite, which is not conducive to the plasticity of the cold heading steel wire rod. If the isothermal temperature is higher, ferrite structure will even appear, which is not conducive to the strength of the cold heading steel wire rod. If the isothermal treatment time is too long, the energy consumption and online time will increase, which is not conducive to efficient production. At the same time, the spacing between the tempered pearlite lamellae increases, the wire rod is over-tempered and softened, and the strength grade of the wire rod is reduced. Therefore, the isothermal temperature and isothermal treatment time of the online salt bath weak isothermal can be further regulated. Preferably, the isothermal temperature of the online salt bath weak isothermal is controlled at 525-555°C, and the isothermal treatment time is controlled at 30-230s to regulate the strength and plasticity matching of the wire rod.

[0025] Preferably, since the wire rod quickly drops from a higher spinning temperature to a lower molten salt temperature after entering the molten salt, the temperature difference is large. Preferably, the front end of the online salt bath weak isothermal salt bath tank controls the molten salt circulation rate to 450-650 t / h, and the molten salt temperature rise is ≤8°C. By preventing the temperature rise from being too high, the wire rod is controlled to complete the isothermal transformation within the target temperature range, and the volume fraction of each phase of the wire rod is regulated.

[0026] Preferably, the rear end of the online salt bath weak isothermal salt bath tank controls the molten salt circulation rate to be 250~450t / h, and the molten salt temperature rise is ≤3°C. The weak isothermal treatment can be completed by controlling the wire rod within the target temperature range to regulate the strength and plasticity matching of the wire rod.

[0027] Preferably, the roller rapid cooling controls the cooling rate of the wire rod to 3-6°C / s, and controls the wire rod to be coiled below 450°C. At this cooling rate, the wire rod can quickly reach the coiling position at a faster cooling rate, preventing excessive softening due to too low a cooling rate and reducing the strength of the cold heading steel wire rod. At the same time, it avoids the cooling rate being too fast so that the temperature of the wire rod reaching the coiling position is too low, resulting in excessive hardening and increased difficulty in coiling. Therefore, the cooling rate of the roller rapid cooling can be further controlled, taking into account both efficient production and the same degree of coiling after the wire rod is coiled.

[0028] Preferably, the roller fast cooling adopts the heat preservation cover to open or the fan is opened at 15% to 40% of the total air volume at the same time, and the total air volume of the fan is 160,000 to 260,000 m 3 / h, the wire rod is transported by rollers at a roller speed of 0.9~1.6m / s, and the cooling speed of the wire rod is controlled by air cooling or weak wind cooling, which is conducive to the efficient production of cold heading steel wire rod.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) In view of the current situation that the hot-rolled wire rods used in existing fastener products are prone to cracking risks during the drawing and cold heading processes of fasteners due to hardenability elements and abnormal structures, the 10.9-grade hot-rolled carbon-reduced annealed cold heading steel wire rod of the present invention is designed with C-Si-Mn carbon chemical composition, and the microstructure type includes a mixed structure composed of tempered pearlite as the main component, a small amount of tempered widmanstattenite which is both strong and tough, and lamellar fused pearlite. Pearlite and widmanstattenite provide matrix strength, and tempering is used to improve the plasticity of pearlite and widmanstattenite structures. Lamellar fused pearlite is used to improve plasticity and reduce annealing difficulty, avoiding the occurrence of bainite abnormal structures. The product tensile strength can reach 880-910MPa, and the cross-sectional shrinkage rate is 57%-61%. It is used in the application fields of manufacturing 10.9-grade high-strength fastener bolts, etc., and at least one annealing process can be reduced, which has good market application prospects.

[0031] (2) In view of the current situation that the hot-rolled wire rods used in fastener products are prone to abnormal structure, low yield and production efficiency by adding elements to improve the hardenability of the material and combining the cooling control means of the Stelmor air cooling line, the manufacturing method of the 10.9 grade hot-rolled carbon reduced annealing cold heading steel plate of the present invention adopts C-Si-Mn carbon chemical composition design and combines online salt bath weak isothermal and roller rapid cooling technology process design, which can promote the high-temperature austenite in the wire rod structure to transform into pearlite with fine lamellar spacing and a small amount of widmanstattenite, and at the same time isothermally tempered to transform into tempered pearlite and tempered widmanstattenite, promote the melting of pearlite lamellae to form lamellar melting pearlite, quickly produce and regulate the strength and plasticity of the hot-rolled wire rod structure, especially improve the plasticity of the cold heading steel wire rod and prevent the wire rod from being over-tempered and softened, which can simplify the manufacturing method, reduce the online time, significantly improve the manufacturing efficiency, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0033] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0034] Figure 2 is the metallographic structure diagram of Example 3 of the present invention;

[0035] Figure 3 It is the metallographic structure diagram of comparative example 6 of the present invention. DETAILED DESCRIPTION

[0036] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0037] A preferred embodiment of the 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.45%, Si: 0.2%, Mn: 0.9%, P: 0.02%, S: 0.019%, and the rest is Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of hot rolling → high temperature wire laying → online salt bath weak isothermal → roller rapid cooling → coiling, specifically:

[0038] The hot rolling process is used to first heat a steel billet with a specification of 160mm×160mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, and then quickly roll it into a wire with a specification of 6.5mm through a rolling line at a high temperature, thereby reducing the wear of the rolling mill of the rolling line and improving the rolling efficiency. At the same time, a higher final rolling temperature and a large final rolling reduction are used to appropriately coarsen the wire grains, so as to prepare the organization for obtaining a proper proportion of pearlite and widmanstatten after spinning. Specifically: the final rolling temperature is controlled to be 987°C, the final rolling reduction is 36%, and the wire grain size is ≤8 levels; the high-temperature spinning process is used to convert the wire exiting the rolling line into a wire rod through a spinning mechanism, and the spinning temperature is controlled to be 965°C. The wire rod is spread on the roller and transported along the roller. The higher spinning temperature is used to appropriately coarsen the austenite grains of the wire rod organization, so that a higher proportion of widmanstatten organization can be more easily obtained.

[0039] The online salt bath weak isothermal adopts a salt bath tank with molten salt inside, which is used to convey the molten salt in the salt bath tank through rollers after the wire rod is spun, so that the wire rod is cooled to the molten salt temperature at a cooling rate of 39°C / s, and the ferrite phase transformation temperature range is quickly skipped at a faster cooling rate, so as to promote the high-temperature austenite in the wire rod structure to transform into pearlite and a small amount of widmanstattenite with fine lamellar spacing, and at the same time isothermally tempered to transform into tempered pearlite and tempered widmanstattenite, and promote the melting of pearlite lamellae to form lamellar melting pearlite, prevent the molten salt temperature from rising too high during the process, and control the wire rod to complete the isothermal transformation within the target temperature range, specifically: the isothermal temperature is controlled at 525°C, the isothermal treatment time is controlled at 30s, the molten salt circulation volume is controlled at 600t / h at the front end of the salt bath tank, and the molten salt temperature rise is ≤8°C, and the molten salt circulation volume is controlled at 450t / h at the rear end of the salt bath tank, and the molten salt temperature rise is ≤3°C.

[0040] The roller fast cooling process uses roller conveyor to convey the wire rod out of the salt bath for fast cooling treatment, so as to prevent the wire rod from being over-tempered and softened and thus reducing the strength grade of the wire rod, and to adjust the strength and plasticity matching of the cold heading steel wire rod. Specifically: the heat preservation cover is opened, and the wire rod out of the salt bath is conveyed by rollers at a roller speed of 0.9 m / s, and the cooling rate of the wire rod is controlled to be 3°C / s until it is transported to the coiling station; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 405°C. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as follows Figure 1 as shown in .

[0041] Comparative Example 1:

[0042] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the manufacturing method differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of low-temperature controlled rolling → low-temperature wire drawing → insulation cooling → coiling, specifically: the final rolling temperature of the low-temperature controlled rolling process is 900°C, the grain size of the wire after rolling is level 9, the wire drawing temperature of the low-temperature wire drawing process is 870°C, the insulation slow cooling adopts the method of conveying the wire rod after wire drawing through a roller conveyor into a heat-insulating cover, completing the phase change at a cooling rate of 2.1°C / s in the cover, the coiling temperature is 400°C, and the cold-heading steel wire rod is obtained after the coiling is off the line.

[0043] Comparative Example 2:

[0044] A method for manufacturing hot-rolled carbon cold-headed steel wire rod, the manufacturing method thereof differs from that of Example 1 in that: the manufacturing method thereof is manufactured according to the process flow of hot rolling → high-temperature wire laying → Stelmor air cooling → roller slow cooling → coiling, specifically: the Stelmor air cooling adopts the method of feeding the wire rod after wire laying into the Stelmor air cooling line, and controlling the total air volume to be 200,000 m 3The 1~4# fans with a flow rate of / h are opened at 75%, so that the wire rod is cooled to 670℃ at a cooling rate of 7.5℃ / s. The fan and the insulation cover are closed for slow cooling on the roller. The wire rod that has passed the Stelmor air cooling is transported by the roller at a speed of 1.3m / s. The cooling rate of the wire rod is controlled to be 0.9℃ / s until it is transported to the coiling station. The coiling temperature is 410℃. After the coiling is off the line, the cold heading steel wire rod is obtained. Embodiment 2:

[0045] A preferred embodiment of the 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.48%, Si: 0.1%, Mn: 0.6%, P: 0.018%, S: 0.018%, and the rest is Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of hot rolling → high temperature wire laying → online salt bath weak isothermal → roller rapid cooling → coiling, specifically:

[0046] The hot rolling process is used to first heat a steel billet with a specification of 160mm×160mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, and then quickly roll it into a wire with a specification of 10mm through a rolling line at a high temperature, thereby reducing the wear of the rolling mill of the rolling line and improving the rolling efficiency. At the same time, a higher final rolling temperature and a large final rolling reduction are used to appropriately coarsen the wire grains, so as to prepare the organization for obtaining a proper proportion of pearlite and widmanstatten after spinning. Specifically: the final rolling temperature is controlled to be 1010°C, the final rolling reduction is 32%, and the wire grain size is ≤8 levels; the high-temperature spinning process is used to convert the wire exiting the rolling line into a wire rod through a spinning mechanism, and the spinning temperature is controlled to be 980°C. The wire rod is spread on the roller and transported along the roller. The higher spinning temperature is used to appropriately coarsen the austenite grains of the wire rod organization, so that a higher proportion of widmanstatten organization can be more easily obtained.

[0047] The online salt bath weak isothermal adopts a salt bath tank with molten salt inside, which is used to convey the molten salt in the salt bath tank through rollers after the wire rod is spun, so that the wire rod is cooled to the molten salt temperature at a cooling rate of 40°C / s, and the ferrite phase transformation temperature range is quickly skipped at a faster cooling rate, so as to promote the high-temperature austenite in the wire rod structure to transform into pearlite with fine lamellar spacing and a small amount of widmanstattensite, and at the same time, isothermally tempered to transform into tempered pearlite and tempered widmanstattensite, and promote the melting of pearlite lamellae to form lamellar melting pearlite, prevent the molten salt temperature from rising too high during the process, and control the wire rod to complete the isothermal transformation within the target temperature range, specifically: the isothermal temperature is controlled at 532°C, the isothermal treatment time is controlled at 95s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 650t / h, and the molten salt temperature rise is ≤8°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 370t / h, and the molten salt temperature rise is ≤3°C.

[0048] The roller fast cooling process uses roller conveyor to quickly cool the wire rod coming out of the salt bath tank to prevent the wire rod from being over-tempered and softened, thereby reducing the strength grade of the wire rod and adjusting the strength and plasticity matching of the cold heading steel wire rod. Specifically: the heat preservation cover is opened, and the total air volume is 160,000 m 3 / h 11~14# fans are turned on at 40% of the total air volume, and the wire rods coming out of the salt bath tank are transported by rollers at a roller speed of 1.4m / s. The cooling rate of the wire rods is controlled to be 4.5℃ / s until they are transported to the coiling station; the coiling process is used to coil the wire rods into coils by means of a coiling drum, and the coiling temperature is 416℃. After packaging and warehousing, the finished cold heading steel wire rods are obtained.

[0049] Comparative Example 3:

[0050] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the manufacturing method of which is different from that of Example 2 in that the final rolling temperature is 950°C, the wire-spinning temperature is 930°C, and the cold-heading steel wire rod is obtained after coiling off the line.

[0051] Comparative Example 4:

[0052] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the manufacturing method of which is different from that of Example 2 in that the final rolling temperature is 1025°C, the wire-spinning temperature is 995°C, and the cold-heading steel wire rod is obtained after coiling off the line. Embodiment 3:

[0053] A preferred embodiment of the 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.46%, Si: 0.15%, Mn: 0.73%, P: 0.018%, S: 0.019%, and the rest is Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of hot rolling → high temperature wire laying → online salt bath weak isothermal → roller rapid cooling → coiling, specifically:

[0054] The hot rolling process is used to first heat a steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, and then quickly roll it into a wire with a specification of 18mm through a rolling line at a high temperature, thereby reducing the wear of the rolling mill of the rolling line and improving the rolling efficiency. At the same time, a higher final rolling temperature and a large final rolling reduction are used to appropriately coarsen the wire grains, so as to prepare the organization for obtaining a proper proportion of pearlite and widmanstatten after spinning. Specifically: the final rolling temperature is controlled to be 992°C, the final rolling reduction is 26%, and the wire grain size is ≤8 levels; the high-temperature spinning process is used to convert the wire exiting the rolling line into a wire rod through a spinning mechanism, and the spinning temperature is controlled to be 970°C. The wire rod is spread on the roller and transported along the roller. The higher spinning temperature is used to appropriately coarsen the austenite grains of the wire rod organization, so that a higher proportion of widmanstatten organization can be more easily obtained.

[0055] The online salt bath weak isothermal adopts a salt bath tank with molten salt inside, which is used to convey the molten salt in the salt bath tank through rollers after the wire rod is spun, so that the wire rod is cooled to the molten salt temperature at a cooling rate of 37°C / s, and the ferrite phase transformation temperature range is quickly skipped at a faster cooling rate, so as to promote the high-temperature austenite in the wire rod structure to transform into pearlite and a small amount of widmanstattenite with fine lamellar spacing, and at the same time isothermally tempered to transform into tempered pearlite and tempered widmanstattenite, and promote the melting of pearlite lamellae to form lamellar melting pearlite, prevent the molten salt temperature from rising too high during the process, and control the wire rod to complete the isothermal transformation within the target temperature range, specifically: the isothermal temperature is controlled at 555°C, the isothermal treatment time is controlled at 230s, the molten salt circulation volume is controlled at 520t / h at the front end of the salt bath tank, and the molten salt temperature rise is ≤8°C, and the molten salt circulation volume is controlled at 250t / h at the rear end of the salt bath tank, and the molten salt temperature rise is ≤3°C.

[0056] The roller fast cooling process uses roller conveyor to fast cool the wire rod coming out of the salt bath tank to prevent the wire rod from being over-tempered and softened, thereby reducing the strength grade of the wire rod and adjusting the strength and plasticity matching of the cold heading steel wire rod. Specifically: the heat preservation cover is opened, and the total air volume is 260,000 m 3 The 11~14# fans with a flow rate of 15% of the total air volume are turned on, and the wire rods coming out of the salt bath are transported by rollers at a roller speed of 1.6m / s. The cooling speed of the wire rods is controlled to be 6℃ / s until they are transported to the coiling station. The coiling process is used to coil the wire rods into coils through the coiling drum. The coiling temperature is 420℃. After packaging and storage, the finished cold heading steel wire rods are obtained. The metallographic structure diagram is as follows Figure 2 as shown in .

[0057] Comparative Example 5:

[0058] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the manufacturing method of which is different from that of Example 3 in that the isothermal temperature is controlled at 500°C, the isothermal treatment time is controlled at 85s, and the cold-heading steel wire rod is obtained after the coil is rolled off the production line.

[0059] Comparative Example 6:

[0060] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the difference between the manufacturing method and the embodiment 3 is that: the isothermal temperature is controlled at 25°C, and the cold-heading steel wire rod is obtained after the coil is rolled off the line. The metallographic structure diagram is as follows Figure 3 as shown in .

[0061] Comparative Example 7:

[0062] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the manufacturing method of which is different from that of Example 3 in that: the isothermal temperature is controlled at 565°C, the isothermal treatment time is controlled at 450s, and the cold-heading steel wire rod is obtained after the coil is rolled off the production line. Embodiment 4:

[0063] A preferred embodiment of the 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.42%, Si: 0.25%, Mn: 0.82%, P: 0.02%, S: 0.02%, and the rest is Fe and unavoidable impurities; the manufacturing method thereof is manufactured according to the process flow of hot rolling → high temperature wire laying → online salt bath weak isothermal → roller rapid cooling → coiling, specifically:

[0064] The hot rolling process is used to first heat a steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, and then quickly roll it into a wire with a specification of 14mm through a rolling line at a high temperature, thereby reducing the wear of the rolling mill of the rolling line and improving the rolling efficiency. At the same time, a higher final rolling temperature and a large final rolling reduction are used to appropriately coarsen the wire grains, so as to prepare the organization for obtaining a proper proportion of pearlite and widmanstatten after spinning. Specifically: the final rolling temperature is controlled to be 980°C, the final rolling reduction is 28%, and the wire grain size is ≤8 levels; the high-temperature spinning process is used to convert the wire exiting the rolling line into a wire rod through a spinning mechanism, and the spinning temperature is controlled to be 960°C. The wire rod is spread on the roller and transported along the roller. The higher spinning temperature is used to appropriately coarsen the austenite grains of the wire rod organization, so that a higher proportion of widmanstatten organization can be more easily obtained.

[0065] The online salt bath weak isothermal adopts a salt bath tank with molten salt inside, which is used to convey the molten salt in the salt bath tank through rollers after the wire rod is spun, so that the wire rod is cooled to the molten salt temperature at a cooling rate of 36°C / s, and the ferrite phase transformation temperature range is quickly skipped at a faster cooling rate, so as to promote the high-temperature austenite in the wire rod structure to transform into pearlite with fine lamellar spacing and a small amount of widmanstattenite, and at the same time, isothermally tempered to transform into tempered pearlite and tempered widmanstattenite, and promote the melting of pearlite lamellae to form lamellar melting pearlite, prevent the molten salt temperature from rising too high during the process, and control the wire rod to complete the isothermal transformation within the target temperature range, specifically: the isothermal temperature is controlled at 546°C, the isothermal treatment time is controlled at 170s, the molten salt circulation volume at the front end of the salt bath tank is controlled to be 450t / h, and the molten salt temperature rise is ≤8°C, and the molten salt circulation volume at the rear end of the salt bath tank is controlled to be 290t / h, and the molten salt temperature rise is ≤3°C.

[0066] The roller fast cooling process uses roller conveyor to fast cool the wire rod coming out of the salt bath tank to prevent the wire rod from being over-tempered and softened, thereby reducing the strength grade of the wire rod and adjusting the strength and plasticity matching of the cold heading steel wire rod. Specifically: the heat preservation cover is opened, and the total air volume is 200,000 m 3The 11~14# fans with a flow rate of / h are turned on at 30% of the total air volume, and the wire rod coming out of the salt bath tank is transported by a roller at a roller speed of 1.2m / s. The cooling rate of the wire rod is controlled to be 5.2℃ / s until it is transported to the coiling station; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the coiling temperature is 390℃. After packaging and warehousing, the finished cold heading steel wire rod is obtained.

[0067] Comparative Example 8:

[0068] A method for manufacturing a hot-rolled carbon cold-heading steel wire rod, the difference between the manufacturing method and Example 4 is that: the manufacturing method is manufactured according to the process flow of hot rolling → high-temperature wire spinning → online salt bath weak isothermal → roller slow cooling → coiling, specifically: the roller slow cooling adopts the fan and the insulation cover to be closed, and the wire rod that has passed the Stelmor air cooling is transported by the roller at a speed of 0.4m / s, and the cooling rate of the wire rod is controlled to be 1.2℃ / s until it is transported to the coiling station, and the coiling temperature is 438℃, and the cold-heading steel wire rod is obtained after the coiling is off the line.

[0069] Comparative Example 9:

[0070] A method for manufacturing hot-rolled carbon cold-headed steel wire rod, the manufacturing method of which is different from that of Example 4 in that: the manufacturing method is manufactured according to the process flow of hot rolling → high-temperature spinning → online salt bath weak isothermal → roller slow cooling → coiling, specifically: the roller fast cooling process adopts the warm hood to open, and the total air volume is 200,000 m 3 The 11~14# fans with a flow rate of / h are turned on at 65% of the total air volume, and the wire rod coming out of the salt bath tank is transported by a roller at a roller speed of 1.1m / s. The cooling rate of the wire rod is controlled to be 7.2℃ / s until it is transported to the coiling station; the coiling temperature is 310℃, and cold heading steel wire rod is obtained after the coiling is off the line.

[0071] The cold heading steel wire rods obtained in the above embodiments and comparative examples were subjected to organizational and performance tests: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0072] Table 1. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0073]

[0074] From the comparison results of Examples 1 to 4 and Comparative Example 1, it can be seen that compared with carbon steel grades, combined with the low-temperature wire drawing and insulation cooling process of the existing Stelmor air-cooled line, abnormal bainite structure will still appear. The present invention, based on the use of medium C-low Si-high Mn, omitting hardenability elements and carbon steel components, promotes the transformation of high-temperature austenite in the wire rod structure into pearlite with fine lamellar spacing and a small amount of widmanstattensite and isothermally tempered to transform it into tempered pearlite and tempered widmanstattensite, and at the same time promotes the melting of pearlite lamellae to form lamellar melting pearlite, which can avoid the situation where the carbon steel increases due to the increase in carbon content, resulting in increased sensitivity and the precipitation of hard and brittle phases during the rapid cooling of the roller, affecting the uniformity of the structure.

[0075] From the comparison results of Examples 1 to 4 and Comparative Example 2, it can be seen that compared with carbon steel grades, the combination of the rapid air cooling and slow cooling process of the existing Stelmor air cooling line under high temperature spinning will significantly increase the brittleness of the cold heading steel wire rod due to the precipitation of the widmanstatten structure along the saturated solid solution crystal plane and the distribution of the widmanstatten structure in the form of flakes or needles. The present invention uses tempering to significantly reduce the dislocation density of the widmanstatten structure to improve the plasticity and toughness properties, and obtain a tempered widmanstatten structure that is both strong and tough, which is mainly tempered pearlite and a small amount of tempered widmanstatten structure. The matrix strength makes up for the strength loss of the band after omitting the hardenability elements. At the same time, the tempered state structure improves the internal stress of the organization and improves the stability of the organization. Combined with a small amount of lamellar melting pearlite formed by the melting of pearlite lamellar layers, the plasticity is improved and the difficulty of annealing is reduced. The product tensile strength can reach 880~910MPa and the cross-sectional shrinkage rate is 57%~61%. It can be used in the manufacture of 10.9 grade high-strength fasteners and bolts and other application fields, which can reduce at least one annealing process and has good market application prospects.

[0076] From the comparison results of Examples 1 to 4 and Comparative Example 3, it can be seen that the lower the spinning temperature, the lower the proportion of tempered widmanstatten in the organization, the strength of the cold heading steel wire rod decreases and the plasticity increases; from the comparison results of Examples 1 to 4 and Comparative Example 4, it can be seen that the higher the spinning temperature, the higher the proportion of tempered widmanstatten in the organization, and the spinning temperature of the wire rod can be further controlled to control the ratio of tempered pearlite to tempered widmanstatten.

[0077] From the comparison results of Examples 1 to 4 and Comparative Example 5, it can be seen that the lower the isothermal temperature and the shorter the isothermal treatment time, the finer the lamellar spacing of the tempered pearlite, which increases the strength of the cold heading steel wire rod and reduces the plasticity. However, from the comparison results of Examples 1 to 4 and Comparative Example 6, it can be seen that if the isothermal temperature is too low, a quenched martensite structure may even appear, causing a significant loss of plasticity. From the comparison results of Examples 1 to 4 and Comparative Example 7, it can be seen that if the isothermal temperature is higher, the lamellar spacing of the tempered pearlite is coarser, which reduces the strength of the cold heading steel wire rod and increases the plasticity. However, if the isothermal temperature is too high, the lamellar spacing of the tempered pearlite is larger, which is not conducive to melting to form lamellar pearlite. The longer the isothermal treatment time, the greater the proportion of lamellar melting pearlite, which reduces the strength of the cold heading steel wire rod and increases the plasticity. The isothermal temperature and isothermal treatment time of the online salt bath weak isothermal can be further regulated to adjust the strength and plasticity matching of the wire rod.

[0078] From the comparison results of Examples 1 to 4 and Comparative Example 8, it can be seen that compared with slow roller cooling, rapid roller cooling can make the wire rod quickly reach the coiling position at a faster cooling speed, thereby preventing excessive softening caused by too low cooling speed and reducing the strength of the cold heading steel wire rod; from the comparison results of Examples 1 to 4 and Comparative Example 9, it can be seen that although increasing the cooling speed of the rapid roller cooling process can improve production efficiency, too fast a cooling speed will cause the temperature of the wire rod to be too low when it reaches the coiling position and over-harden, resulting in serious coil misalignment, which is not conducive to packaging and transportation.

[0079] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, the steel billet before hot rolling can be produced by the process of converter smelting, refining and continuous casting. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.42% to 0.48%, Si: 0.1% to 0.25%, Mn: 0.6% to 0.9%, P≤0.020%, S≤0.020%, and the rest are Fe and unavoidable impurities; its microstructure includes a mixed structure consisting of 70% to 76% by volume of tempered pearlite, 22% to 28% by volume of tempered widmanstattenite, and the rest of the lamellar melt pearlite, and its manufacturing method includes: The wire rod is produced based on the chemical composition of the 10.9 grade hot-rolled carbon reduced annealed cold heading steel wire rod, the wire rod is spun into a wire rod at a spinning temperature of ≥960°C, the wire rod is subjected to online salt bath weak isothermal treatment, the wire rod is cooled to the molten salt temperature at a cooling rate of ≥36°C / s, the high-temperature austenite in the wire rod structure is transformed into pearlite with fine lamellar spacing and a small amount of widmanstattenite, and isothermally tempered to be transformed into tempered pearlite and tempered widmanstattenite, and the pearlite lamellar melting is promoted to form lamellar melting pearlite, and finally the cold heading steel wire rod is subjected to roller rapid cooling to obtain a mixed structure of tempered pearlite, tempered widmanstattenite and lamellar melting pearlite with a microstructure of 70% to 76% by volume, the isothermal temperature of the online salt bath weak isothermal treatment is controlled at 525 to 555°C, and the isothermal treatment time is controlled at 30 to 230s.

2. The 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 75-100 nm.

3. The 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 6.5-18.0 mm, a tensile strength of 880-910 MPa, and a cross-sectional shrinkage of 57%-61%.

4. A method for manufacturing a 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod, characterized in that: The manufacturing method thereof comprises: A wire rod is produced based on the chemical composition of the 10.9 grade hot-rolled carbon reduced annealed cold heading steel wire rod as described in claim 1, the wire rod is spun into a wire rod at a spinning temperature of ≥960°C, the wire rod is subjected to weak isothermal treatment in an online salt bath, and the wire rod is cooled to a molten salt temperature at a cooling rate of ≥36°C / s, so that the high-temperature austenite in the wire rod structure is transformed into pearlite and widmanstattenite with fine lamellar spacing, and is isothermally tempered to transform into tempered pearlite and tempered widmanstattenite, and the pearlite lamellae are melted to form lamellar fused pearlite, and finally the wire rod is rapidly cooled by a roller to be made into a cold heading steel wire rod having a microstructure including a mixed structure consisting of 70% to 76% by volume of tempered pearlite, 22% to 28% by volume of tempered widmanstattenite and lamellar fused pearlite.

5. The method for manufacturing 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 4, characterized in that: The wire rod is produced by hot rolling, the final rolling temperature is controlled to be 980-1010° C., the final rolling reduction is 26%-36%, and the wire rod grain size is ≤8 levels.

6. The method for manufacturing 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 5, characterized in that: The spinning temperature is ≤980°C.

7. The method for manufacturing the 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to any one of claims 4 to 6, characterized in that: The isothermal temperature of the online salt bath weak isothermal is controlled at 525-555° C., and the isothermal treatment time is controlled at 30-230 s.

8. The method for manufacturing 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 7, characterized in that: The front end of the online weakly isothermal salt bath tank controls the molten salt circulation volume to be 450-650t / h, and the molten salt temperature rise is ≤8°C; the rear end of the salt bath tank controls the molten salt circulation volume to be 250-450t / h, and the molten salt temperature rise is ≤3°C.

9. The method for manufacturing 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 7, characterized in that: The roller fast cooling controls the cooling speed of the wire rod to be 3-6°C / s, and controls the wire rod to be coiled at below 450°C.

10. The method for manufacturing 10.9 grade hot-rolled carbon-reduced annealed cold heading steel wire rod according to claim 9, characterized in that: The roller fast cooling adopts the method of opening the heat preservation cover or simultaneously opening the fan at 15% to 40% of the total air volume. The total air volume of the fan is 160,000 to 260,000 m3 / h, and the wire rod is transported by the roller at a roller speed of 0.9 to 1.6 m / s.