Electrolyte and lithium-sulfur battery

Through the synergistic effect of high salt concentration co-ion effects and high C/O ratio ether solvents, combined with benzene thiol compounds and nitrates, the dissolution of LiPSs is inhibited, solving the problems of electrolyte corrosion and high temperature safety of lithium-sulfur batteries, and improving The overall performance of the battery.

CN118380656BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410805974.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

During the charge and discharge process of lithium-sulfur batteries, the electrolyte is seriously corroded due to the dissolution and self-discharge effect of LiPSs, low Coulombic efficiency, and poor safety in high-temperature environments.

Method used

The co-ion effect of high salt concentration and the synergistic effect of ether solvents with high C/O ratio and low polarity solvents are used to suppress the dissolution of LiPSs and form stable oligomers through the combination of benzenethiol compounds and nitrates. , improve the safety of lithium metal, and add ester co-solvents and fluorine-containing compounds to the electrolyte to improve the overall performance of the electrolyte.

Benefits of technology

It effectively inhibits the dissolution of LiPSs and electrolyte corrosion, improves the safety of lithium metal in high temperature environments, and improves the cycle performance, rate performance and safety performance of lithium-sulfur batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and specifically relates to an electrolyte and a lithium-sulfur battery. The electrolyte includes a first lithium salt, a second lithium salt, a first solvent, a second solvent and an additive; wherein the first lithium salt and the second lithium salt are different substances; the first solvent is an ether compound, and the C / O molar ratio of the ether compound is ≥4; the dipole moment of the second solvent is ≤6.2; the additive includes a benzenethiol compound and a nitrate. On the one hand, the coordination effect of the solvent with lower polarity and lithium ions is weak, and the high concentration of common ion effect formed by the double lithium salt in the electrolyte can effectively inhibit the dissolution and self-discharge effect of LiPSs in the electrolyte; on the other hand, the solubility of LiPSs in ether solvents with higher C / O molar ratio is lower, which can further effectively inhibit the dissolution of LiPSs, thereby alleviating the electrolyte corrosion phenomenon in lithium-ion batteries and improving the safety of lithium metal in high temperature environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to an electrolyte and a lithium-sulfur battery. Background Art

[0002] With the widespread application of outdoor smart electronic devices (such as drones), more stringent requirements are placed on high energy density, low cost, and high and low temperature rechargeable batteries. Lithium-sulfur (Li-S) batteries are regarded as one of the most promising high energy density alternatives due to the high specific capacity of their electrodes. However, during the charge and discharge process, the complex Li-S chemistry involves the formation of lithium polysulfide intermediates (LiPSs), which leads to the shuttle effect during the charge and discharge process.

[0003] For sulfur electrodes, carbonates are a common type of electrolyte, and most conventional electrolytes on the market are carbonate electrolytes, which are relatively low in cost. However, carbonate electrolytes have poor compatibility with metallic lithium and react with lithium to form an organic SEI film of alkyl lithium carbonate (ROCO2Li). This SEI film cannot withstand the volume expansion of repeated lithium deposition, so it will continue to thicken and cause the lithium negative electrode to fail quickly. During the battery charging and discharging process, LiPS x (Li2S x , x = 4~8) is easily soluble in ether electrolyte, separated from the positive electrode to the negative electrode, and chemically reduced to LiPS x (Li2S x ,x=3), and then return to the positive electrode to be oxidized to LiPSs with x=4~8; due to the difference in chemical potential and concentration, this LiPSs shuttles between the two electrodes, resulting in several disadvantages: low sulfur utilization, difficult electron / ion transfer, low Coulomb efficiency, and severe corrosion. Summary of the invention

[0004] The present invention provides an electrolyte and a lithium-sulfur battery, which aims to inhibit the dissolution of LiPSs in the electrolyte through the common ion effect of high salt concentration and the synergistic effect of high C / O ratio solvents, low polarity solvents, etc., improve the safety of lithium metal in high temperature environments, and solve the problems of serious electrolyte corrosion and low coulomb efficiency in existing lithium-ion batteries.

[0005] In one aspect, the present invention provides an electrolyte comprising a first lithium salt, a second lithium salt, a first solvent, a second solvent and an additive;

[0006] Wherein, the first lithium salt and the second lithium salt are different substances;

[0007] The first solvent is an ether compound, and the C / O molar ratio of the ether compound is ≥4;

[0008] The dipole moment of the second solvent is ≤6.2;

[0009] The additive comprises a benzenethiol compound and a nitrate, and the molar ratio of the benzenethiol compound to the nitrate is 1:0.1-30.

[0010] In some embodiments, the molar ratio of the first lithium salt, the second lithium salt, the first solvent and the second solvent is 1:1-10:0.5-20:0.5-20.

[0011] In some embodiments, the first lithium salt and the second lithium salt include any two of lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium hexafluorophosphate.

[0012] In some embodiments, the first solvent includes one or more of isopropyl ether, isobutyl ether, butyl ether, ethyl butyl ether, amyl ether, n-hexyl ether, heptyl ether, dioctyl ether, tert-butyl ether, methyl butyl ether, sec-butyl ether, ethylene glycol dibutyl ether, isopentyl ether and isobutyl tert-butyl ether.

[0013] In some embodiments, the second solvent comprises one or more of tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, furan, 2-(tetrahydrofuran-3-yl)acetonitrile, tetrahydropyranone, 3-ketopyran, tetrahydropyran-2-ol, 4-aldehyde tetrahydropyran, tetrahydropyran-3-carbonitrile, tetrahydropyran-4,4-dicarbonitrile, 2H-benzopyran-3-carbonitrile, (tetrahydropyran-4-ylidene)acetonitrile, 2H-pyran-3(6H)-one and 2-tetrahydropyran-3-ylideneacetonitrile.

[0014] In some embodiments, the electrolyte further includes an ester co-solvent.

[0015] In some embodiments, the molar ratio of the ester co-solvent to the first lithium salt is 0.25-10:1.

[0016] In some embodiments, the ester co-solvent includes one or more of ethylene carbonate, vinylene carbonate, vinyl sulfite, bisfluoroethylene carbonate and fluoroethylene carbonate.

[0017] In some embodiments, the electrolyte further includes a fluorine-containing compound.

[0018] In some embodiments, the molar ratio of the fluorine-containing compound to the first lithium salt is 1.5-30:1.

[0019] In some embodiments, the fluorine-containing compound includes one or more of polyfluoro, flutir, desflurane, sevoflurane, perfluorocyclic ether, trifluoroacetonitrile ether, hexafluoroisopropyl methyl ether, methyl nonafluorobutyl ether, perfluoropropyl vinyl ether and eicosyl-15-crown-5-ether.

[0020] In some embodiments, the mass percentage of the additive in the electrolyte is 0.05% to 15%.

[0021] In some embodiments, the benzenethiol compound includes one or more of benzenethiol, pentafluorobenzenethiol, 3-aminobenzenethiol, 4-nitrobenzenethiol, 3-ethylbenzenethiol, 2-isopropylbenzenethiol, 4-methylthiobenzenethiol, 2,6-difluorobenzenethiol, 2-trifluoromethylbenzenethiol, 5-fluoro-2-methylbenzenethiol, 4-(4-fluoro-phenoxy)-benzenethiol, 1,4-phenyldithiol, 1,4-benzenedimethanethiol and 1,2-benzenedithiol.

[0022] In some embodiments, the nitrate includes one or more of potassium nitrate, cesium nitrate, nickel nitrate, zinc nitrate, manganese nitrate, indium nitrate, rubidium nitrate, cesium nitrate, magnesium nitrate, chromium nitrate, copper nitrate, lithium nitrate and cobalt nitrate.

[0023] On the other hand, the present invention further provides a lithium-sulfur battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte is the electrolyte in any of the above embodiments.

[0024] The present invention provides an electrolyte, comprising a first lithium salt, a second lithium salt, a first solvent, a second solvent and an additive; wherein the first lithium salt and the second lithium salt are different substances; the first solvent is an ether compound, and the C / O molar ratio of the ether compound is ≥2; the dipole moment of the second solvent is ≤6.2; the additive comprises a benzenethiol compound and a nitrate, and the molar ratio of the benzenethiol compound to the nitrate is 1:0.1~30. The electrolyte provided by the present invention combines two different lithium salts with components such as an ether solvent with a high C / O molar ratio and a low polarity solvent. On the one hand, the coordination effect of the solvent with a lower polarity and lithium ions is weak, and the high concentration of common ion effect is formed by combining with the double lithium salt in the electrolyte, which can effectively inhibit the dissolution and self-discharge effect of LiPSs in the electrolyte; on the other hand, the solubility of LiPSs in the ether solvent with a higher C / O molar ratio is lower, which can further effectively inhibit the dissolution of LiPSs, thereby alleviating the electrolyte corrosion phenomenon in the lithium ion battery and improving the safety of lithium metal in a high temperature environment. In addition, the S in the sulfur electrode will be converted into Li2S in the electrolyte. x (4≤x≤8), the benzenethiol in the electrolyte can not only combine with S to form oligomers, but also with Li + 、e - Combine to form Li2-benzenethiol and Li2S; at the beginning of the charging process, the insoluble Li2S is converted to Li2S x (2≤x<4), with the increase of sulfur atoms, Li2S x (4≤x≤8) begins to dissolve into the electrolyte and combines with the phenylsulfate radicals in the oligomer to generate Li + and e− Then two phenyl disulfide free radicals combine to form a tetrasulfide dimer, which can form a covalent SS bond with 2 to 4 S atoms to become an oligomer; during the discharge process, the oligomer is lithiated, and with the formation and breaking of the SS bond, the sulfur undergoes a reversible chemical reaction, which can inhibit the dissolution of polysulfide in the electrolyte; the sulfur free radical has more freedom and position to form the SS bond, and SS is more stable than the elemental S. The electrolyte of the present invention is conducive to improving the comprehensive performance of the electrolyte through the coordinated cooperation of the first lithium salt, the second lithium salt, the first solvent, the second solvent and the additive, thereby improving the comprehensive performance of the battery. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, "several" means two or more than two, unless otherwise specifically defined. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.

[0027] According to one aspect of the present invention, the present invention provides an electrolyte, comprising a first lithium salt, a second lithium salt, a first solvent, a second solvent and an additive;

[0028] wherein the first lithium salt and the second lithium salt are different substances;

[0029] The first solvent is an ether compound, and the C / O molar ratio of the ether compound is ≥4;

[0030] The dipole moment of the second solvent is ≤ 6.2;

[0031] The additive comprises a benzenethiol compound and a nitrate, and the molar ratio of the benzenethiol compound to the nitrate is 1:0.1-30.

[0032] On the one hand, solvents with lower polarity have weaker coordination effects with lithium ions, and combined with the high concentration of co-ion effect formed by the double lithium salt in the electrolyte, the dissolution and self-discharge effect of LiPSs in the electrolyte can be effectively inhibited; on the other hand, LiPSs have lower solubility in ether solvents with a higher C / O molar ratio, which can further effectively inhibit the dissolution of LiPSs, thereby alleviating the electrolyte corrosion phenomenon in lithium-ion batteries and improving the safety of lithium metal in high temperature environments.

[0033] It is understood that the C / O molar ratio of the ether compound can be any value such as 4, 6, 8, 10, or a range between any two values; the dipole moment can be any value such as 0.5, 1, 1.5, 2, 4, 6, or a range between any two values. When the C / O molar ratio of the first solvent ether compound and the dipole moment of the second solvent meet the above value ranges, the polarity of the solvent can be ensured to be low, which has a more ideal effect on inhibiting the dissolution of LiPSs in the electrolyte.

[0034] In some embodiments, the molar ratio of the benzenethiol compound to the nitrate can be, for example but not limited to, 1:0.1, 1:1, 1:2, 1:5, 1:10, 1:15, 1:20, 1:25 or 1:30, or any range therebetween.

[0035] The sulfur in the sulfur electrode will be converted into Li2S in the electrolyte x (4≤x≤8), benzenethiol can not only combine with S to form oligomers, but also with Li + 、e - Combine to form Li2-benzenethiol and Li2S; at the beginning of the charging process, the insoluble Li2S is converted to Li2S x (2≤x<4), with the increase of sulfur atoms, Li2S x (4≤x≤8) begins to dissolve into the electrolyte and combines with the phenylsulfate radicals in the oligomer to generate Li + and e − Then two benzene disulfide radicals combine to form a tetrasulfide dimer, which can form covalent SS bonds with 2 to 4 S atoms to become an oligomer; during the discharge process, the oligomer is lithiated, and with the formation and breaking of SS bonds, sulfur undergoes a reversible chemical reaction, which can inhibit the dissolution of polysulfides in the electrolyte; sulfur radicals have more freedom and positions to form SS bonds, and SS is more stable than elemental S.

[0036] In some embodiments, the mass percentage of the additive in the electrolyte is 0.05% to 15%. It is understood that the mass percentage of the additive in the electrolyte can be any value of 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2.5%, 5%, 7.5%, 10%, 15%, or a range between any two values.

[0037] In some embodiments, the benzenethiol compound includes one or more of benzenethiol, pentafluorobenzenethiol, 3-aminobenzenethiol, 4-nitrobenzenethiol, 3-ethylbenzenethiol, 2-isopropylbenzenethiol, 4-methylthiobenzenethiol, 2,6-difluorobenzenethiol, 2-trifluoromethylbenzenethiol, 5-fluoro-2-methylbenzenethiol, 4-(4-fluoro-phenoxy)-benzenethiol, 1,4-phenyldithiol, 1,4-benzenedimethanethiol and 1,2-benzenedithiol.

[0038] In some embodiments, the nitrate includes one or more of potassium nitrate, cesium nitrate, nickel nitrate, zinc nitrate, manganese nitrate, indium nitrate, rubidium nitrate, cesium nitrate, magnesium nitrate, chromium nitrate, copper nitrate, lithium nitrate, and cobalt nitrate.

[0039] In some embodiments, the molar ratio of the first lithium salt, the second lithium salt, the first solvent, and the second solvent is 1:1-10:0.5-20:0.5-20. In some embodiments, the molar ratio of the first lithium salt, the second lithium salt, the first solvent, and the second solvent may be, but is not limited to, 1:1:0.5:0.5, 1:2:3:3, 1:3:5:5, 1:5:10:10, 1:8:15:12, 1:10:15:20, 1:10:20:16, and the like.

[0040] The content of the first lithium salt and the second lithium salt in the electrolyte will affect the conductivity of the electrolyte. If the lithium salt content is too low, the electrolyte conductivity will be low, and the polarization voltage of lithium plating / stripping will increase. If the lithium salt content is too high, the electrolyte viscosity will be too high, and the lithium ion migration rate will decrease significantly. Ether solvents are additives in the electrolyte. If the content of ether solvents is too high, the dissolution rate of lithium salts in the electrolyte may be too low, resulting in Li + The coordination number with ether solvent is too high, the free solvent increases, Li + The coordination number with the anion decreases, and the polarization voltage increases accordingly. If the content of the ether solvent is too low, it cannot inhibit the dissolution of LiPSs in the electrolyte. When the molar ratio of the first lithium salt, the second lithium salt, the first solvent, and the second solvent meets the above range, the concentration of LiPSs in the electrolyte and the polarization voltage of the electrolyte can be within the ideal range.

[0041] In some embodiments, the first lithium salt and the second lithium salt include any two of lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF4), lithium difluorooxalatoborate (LiDFOB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium hexafluorophosphate (LiPF6).

[0042] In some embodiments, the first solvent includes one or more of isopropyl ether, isobutyl ether, butyl ether, ethyl butyl ether, amyl ether, n-hexyl ether, heptyl ether, dioctyl ether, tert-butyl ether, methyl butyl ether, sec-butyl ether, ethylene glycol dibutyl ether, isopentyl ether and isobutyl tert-butyl ether.

[0043] In some embodiments, the second solvent includes one or more of tetrahydrofuran, tetrahydropyran, 2-methyltetrahydrofuran, furan, 2-(tetrahydrofuran-3-yl)acetonitrile, tetrahydropyranone, 3-ketopyran, tetrahydropyran-2-ol, 4-aldehyde tetrahydropyran, tetrahydropyran-3-carbonitrile, tetrahydropyran-4,4-dicarbonitrile, 2H-benzopyran-3-carbonitrile, (tetrahydropyran-4-ylidene)acetonitrile, 2H-pyran-3(6H)-one and 2-tetrahydropyran-3-ylideneacetonitrile.

[0044] In some embodiments, the electrolyte further includes an ester co-solvent.

[0045] In some embodiments, the molar ratio of the ester co-solvent to the first lithium salt is 0.25 to 10: 1. It is understood that the molar ratio of the ester co-solvent to the first lithium salt is any value of 0.25: 1, 0.5: 1, 1: 1, 3: 1, 5: 1, 7: 1, 10: 1 or a range between any two values.

[0046] Ester co-solvents have high solubility. Adding a small amount of ester co-solvents to the electrolyte can increase the concentration of dissolved ions in the electrolyte and increase the ion transfer rate in the electrolyte, thereby reducing the internal resistance of the battery. If the amount of ester co-solvent added is too high, it is easy to cause the electrolyte and the negative electrode lithium metal to be incompatible. When the amount of ester co-solvent added meets the above range of values, it can ensure that the internal resistance of the battery is reduced as much as possible on the basis of compatibility between the electrolyte and the negative electrode lithium metal, and improve the conductivity.

[0047] In some embodiments, the ester co-solvent includes one or more of ethylene carbonate, vinylene carbonate, vinyl sulfite, bisfluoroethylene carbonate, and fluoroethylene carbonate.

[0048] In some embodiments, the electrolyte further includes a fluorine-containing compound.

[0049] The powerful solvent formed by fluorine-containing compounds can not only alleviate the problem that low-polarity solvents are prone to form peroxides in high temperature and oxygen-rich environments, playing a balancing role, but also can form SEI on the lithium negative electrode side and organic and inorganic CEI on the sulfur positive electrode side through reduction decomposition, forming a good passivation layer at the interface between the electrode and the electrolyte.

[0050] In some embodiments, the molar ratio of the fluorine-containing compound to the first lithium salt is 1.5 to 30: 1. It is understood that the molar ratio of the fluorine-containing compound to the first lithium salt can be any value of 1.5: 1, 5: 1, 10: 1, 15: 1, 20: 1, 25: 1, 30: 1 or a range between any two values. When the amount of the fluorine-containing compound added satisfies the above range, it can ensure that the electrolyte has an ideal antioxidant capacity, especially in a high temperature and oxygen-rich environment.

[0051] In some embodiments, the fluorine-containing compound includes one or more of polyfluoro, flutir, desflurane, sevoflurane, perfluorocyclic ether, trifluoroacetonitrile ether, hexafluoroisopropyl methyl ether, methyl nonafluorobutyl ether, perfluoropropyl vinyl ether and eicosyl-15-crown-5-ether.

[0052] In some embodiments, the electrolyte may include a first lithium salt, a second lithium salt, a first solvent, a second solvent, an ester co-solvent and a fluorine-containing compound at the same time. When the molar ratio of the above components satisfies 1:1~10:0.5~20:0.5~20:0.25~10:1.5~3, the electrolyte can obtain relatively ideal comprehensive performance.

[0053] According to another aspect of the present invention, the present invention further provides a lithium-sulfur battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte is the electrolyte in any of the above embodiments.

[0054] The lithium-sulfur battery of the present invention has excellent cycle performance, rate performance and safety performance.

[0055] The electrolyte and lithium-sulfur battery provided by the present invention are described below in conjunction with specific embodiments:

[0056] Example 1

[0057] This embodiment provides an electrolyte, which is prepared by the following method:

[0058] S1. Mix LiFSI, LiBF4, isopropyl ether, tetrahydrofuran, ethylene carbonate, and trifluoroacetonitrile ether in a molar ratio of 1:3:2.5:2.5:0.8:8 to obtain a mixed solution;

[0059] S2. Add 0.75% by mass of additives to the mixed solution, wherein the additives include 1,4-benzenedimethylenethiol and potassium nitrate, and the molar ratio of 1,4-benzenedimethylenethiol to potassium nitrate is 1:5. Mix well to obtain an electrolyte.

[0060] The electrolyte obtained by the above method is further prepared into a battery through the following steps:

[0061] 1) Preparation of positive electrode sheet: PAN / S positive electrode material, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly at a mass ratio of 97:2:0.5:0.5 to form a lithium-ion battery positive electrode slurry with a certain viscosity, coated on the aluminum foil for current collector, dried at 70°C and cold pressed; then trimmed, cut and slit, and dried at 65°C for 12 hours under vacuum to produce a lithium metal battery positive electrode sheet that meets the requirements;

[0062] 2) The negative electrode uses a 6μm thick copper foil purchased from the market, and a copper-lithium composite strip coated with lithium on both sides (the thickness of lithium is 50μm); after trimming, cutting and slitting, it is made into a lithium metal battery negative electrode sheet that meets the requirements;

[0063] 3) Preparation of lithium metal button battery: The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are stacked to form a CR2032 button lithium metal battery with a capacity of 500 mAh, and the above electrolyte is injected to complete the battery production.

[0064] Example 2

[0065] The steps for preparing the electrolyte and the battery in Example 2 are the same as those in Example 1, except that the types of ether compounds used are different, and the amount of the second lithium salt added is different. For the selection of specific materials, see Table 1.

[0066] Example 3

[0067] The steps for preparing the electrolyte and the battery in Example 3 are the same as those in Example 1, except that different types of ether compounds, low-polarity solvents, ester co-solvents and fluorine-containing compounds are used, and the amount of the second lithium salt added is different. For the selection of specific materials, see Table 1.

[0068] Example 4

[0069] The steps for preparing the electrolyte and the battery in Example 4 are the same as those in Example 1, except that the types of the second lithium salt, the ether compound, the low-polarity solvent, the ester co-solvent and the fluorine-containing compound used are different, as well as the amount of the ether compound added. For specific material selection, see Table 1.

[0070] Example 5

[0071] The steps for preparing the electrolyte and the battery in Example 5 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of ether compound added. For specific material selection, see Table 1.

[0072] Example 6

[0073] The steps for preparing the electrolyte and the battery in Example 6 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of low-polarity solvent added. For specific material selection, see Table 1.

[0074] Example 7

[0075] The steps for preparing the electrolyte and the battery in Example 7 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, and the amount of low-polarity solvent added is different. For specific material selection, see Table 1.

[0076] Example 8

[0077] The steps for preparing the electrolyte and the battery in Example 8 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of ester co-solvent added is different. For specific material selection, see Table 1.

[0078] Example 9

[0079] The steps for preparing the electrolyte and the battery in Example 9 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of ester co-solvent added. For specific material selection, see Table 1.

[0080] Example 10

[0081] The steps for preparing the electrolyte and the battery in Example 10 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of fluorine-containing compound added. For specific material selection, see Table 1.

[0082] Embodiment 11

[0083] The steps for preparing the electrolyte and the battery in Example 11 are the same as those in Example 1, except that the types of the second lithium salt, ether compound, low-polarity solvent, ester co-solvent and fluorine-containing compound used are different, as well as the amount of fluorine-containing compound added. For specific material selection, see Table 1.

[0084] Example 12

[0085] The steps for preparing the electrolyte and the battery in Example 12 are the same as those in Example 1, except that no additives are added. For the selection of specific materials, see Table 1.

[0086] Example 13

[0087] The steps for preparing the electrolyte and the battery in Example 13 are the same as those in Example 1, except that no ester co-solvent is added. For the selection of specific materials, see Table 1.

[0088] Embodiment 14

[0089] The steps for preparing the electrolyte and the battery in Example 14 are the same as those in Example 1, except that no fluorine-containing compound is added. For the selection of specific materials, see Table 1.

[0090] Embodiment 15

[0091] The steps for preparing the electrolyte and the battery in Example 15 are the same as those in Example 1, except that no ester co-solvent and fluorine-containing compound are added. For the selection of specific materials, see Table 1.

[0092] Comparative Example 1

[0093] The steps for preparing the electrolyte and the battery in Comparative Example 1 are the same as those in Example 1, except that the second lithium salt is not added. For the selection of specific materials, see Table 1.

[0094] Comparative Example 2

[0095] The steps for preparing the electrolyte and the battery in Comparative Example 2 are the same as those in Example 1, except that no ether compound is added. For the selection of specific materials, see Table 1.

[0096] Comparative Example 3

[0097] The steps for preparing the electrolyte and the battery in Comparative Example 3 are the same as those in Example 1, except that no low-polarity solvent is added. For the selection of specific materials, see Table 1.

[0098] Comparative Example 4

[0099] The steps for preparing the electrolyte and the battery in Comparative Example 4 are the same as those in Example 1, except that methyl ethyl ether is used as the first solvent. For the selection of specific materials, see Table 1.

[0100] Comparative Example 5

[0101] The steps for preparing the electrolyte and the battery in Comparative Example 5 are the same as those in Example 1, except that 1,3,2-Dioxathiolane,4,5-dimethyl-,2,2-dioxide (DTD2M, CAS: 4440-89-5) is used as the second solvent. For the selection of specific materials, see Table 1.

[0102] The electrolyte additive components of Examples 1 to 15 and Comparative Examples 1 to 5 are shown in Table 1.

[0103] Table 1 Electrolyte additive components

[0104] Group The first lithium salt Second lithium salt Ether compounds C / O molar ratio Low polarity solvent Dipole moment Ester co-solvent Fluorinated compounds Molar ratio of components Benzenethiol Nitrates Molar Ratio Additive amount Example 1 LiFSI LiBF4 Isopropyl ether 6 Tetrahydrofuran 2.01 Ethylene carbonate Trifluoroacetonitrile ether 1:3:2.5:2.5:0.8:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:5 0.75% Example 2 LiFSI LiBF4 Isobutyl ether 8 Tetrahydrofuran 2.01 Ethylene carbonate Trifluoroacetonitrile ether 1:1:2.5:2.5:0.8:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:5 0.75% Example 3 LiFSI LiBF4 Butyl ether 8 Tetrahydropyran 1.63 Ethylene carbonate Flutir 1:10:2.5:2.5:0.8:8 3-Aminobenzenethiol Potassium Nitrate 1:5 0.75% Example 4 LiFSI LiBF4 Tert-butyl ether 8 2-Methyltetrahydrofuran 1.65 Ethylene carbonate Desflurane 1:3:0.5:2.5:0.8:8 4-Nitrobenzenethiol Potassium Nitrate 1:0.1 0.05% Example 5 LiFSI LiPF6 Tert-butyl ether 8 Furan 0.75 Vinylene carbonate Desflurane 1:3:20:2.5:0.8:8 4-Nitrobenzenethiol Potassium Nitrate 1:0.5 0.10% Example 6 LiFSI LiPF6 Ethylene glycol dibutyl ether 5 2-(Tetrahydrofuran-3-yl)acetonitrile 4.58 Vinylene carbonate Sevoflurane 1:3:2.5:0.5:0.8:8 2,6-Difluorobenzenethiol, Potassium Nitrate 1:1 0.15% Example 7 LiFSI LiDFOB Isopropyl ether 6 Tetrahydropyrone 1.85 Ethylene bis(fluorocarbonate) Perfluorocyclic ether 1:3:2.5:20:0.8:8 3-Aminobenzenethiol Potassium Nitrate 1:1 1.00% Example 8 LiFSI LiDFOB Amyl ether 10 3-Ketopyran 3.13 Vinylene carbonate Perfluorocyclic ether 1:3:2.5:2.5:0.25:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:10 2.00% Example 9 LiFSI LiTFSI Isobutyl tert-butyl ether 8 Tetrahydropyran-2-ol 2.18 Vinylene carbonate Desflurane 1:3:2.5:2.5:10:8 1,2-Benzenedithiol Potassium Nitrate 1:15 5.00% Example 10 LiFSI LiBF4 Isopropyl ether 6 4-Formyltetrahydropyran 2.53 Vinylene carbonate Sevoflurane 1:3:2.5:2.5:0.8:1.5 3-Ethylbenzenethiol Potassium Nitrate 1:20 10.00% Embodiment 11 LiFSI LiBF4 Isobutyl ether 8 Tetrahydropyran-3-carbonitrile 3.95 Fluoroethylene carbonate Trifluoroacetonitrile ether 1:3:2.5:2.5:0.8:30 Pentafluorobenzenethiol Potassium Nitrate 1:30 15.00% Example 12 LiFSI LiBF4 Isopropyl ether 6 Tetrahydrofuran 7.59 Ethylene carbonate Trifluoroacetonitrile ether 1:3:2.5:2.5:0.8:8 - - - - Example 13 LiFSI LiBF4 Isopropyl ether 6 Tetrahydrofuran 2.01 - Trifluoroacetonitrile ether 1:3:2.5:2.5:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:05 0.75% Embodiment 14 LiFSI LiBF4 Isopropyl ether 6 Tetrahydrofuran 2.01 Ethylene carbonate - 1:3:2.5:2.5:0.8 1,4-Benzenedimethanethiol Potassium Nitrate 1:05 0.75% Embodiment 15 LiFSI LiBF4 Isopropyl ether 6 Tetrahydrofuran 2.01 - - 1:3:2.5:2.5 1,4-Benzenedimethanethiol Potassium Nitrate 1:05 0.75% Comparative Example 1 LiFSI - Isopropyl ether 6 Tetrahydrofuran 2.01 Ethylene carbonate Trifluoroacetonitrile ether 4:2.5:2.5:0.8:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:5 0.75% Comparative Example 2 LiFSI LiBF4 - - Tetrahydrofuran 2.01 - - 1:3:2.5 - - - - Comparative Example 3 LiFSI LiBF4 Isopropyl ether 6 - - - - 1:3:2.5 - - - - Comparative Example 4 LiFSI LiBF4 Methyl ethyl ether 3 Tetrahydrofuran 2.01 Ethylene carbonate Trifluoroacetonitrile ether 1:3:2.5:2.5:0.8:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:5 0.75% Comparative Example 5 LiFSI LiBF4 Isopropyl ether 6 DTD2M 6.54 Ethylene carbonate Trifluoroacetonitrile ether 1:3:2.5:2.5:0.8:8 1,4-Benzenedimethanethiol Potassium Nitrate 1:5 0.75%

[0105] The batteries prepared in Examples 1 to 15 and Comparative Examples 1 to 5 were subjected to electrical performance tests, and the testing method included the following steps:

[0106] (1) First effect: At 25±3℃, charge at 0.05C constant current to 3.0V, charge at 3.0V constant voltage to cut-off current 0.05C, record the charge capacity as C1, then discharge at 0.05C constant current to 1.0V, record the discharge capacity as D1; ​​first effect = (D1 / C1) × 100%;

[0107] (2) Capacity retention rate at the 150th cycle (normal temperature 25°C): At 25±3°C, charge the battery at a constant current of 0.33C to 3.0V, charge it at a constant voltage of 3.0V to a cut-off current of 0.05C, and then discharge it at a constant current of 1C to 1.0V. The discharge capacity is recorded as C1. Repeat the charge and discharge steps for 150 cycles to obtain the discharge capacity C1 at the Nth cycle. N , Nth cycle capacity retention rate = (C N / C1)×100%;

[0108] (3) Average Coulombic efficiency of the first 150 cycles (normal temperature 25°C): Same as the test in step 2, the calculation method is as follows: Coulombic efficiency of each cycle CE = discharge capacity / charge capacity × 100%, average Coulombic efficiency of the first N cycles CE = SUM (CE1~CE N ) / N×100%;

[0109] (4) Capacity retention rate at the 100th cycle (high temperature 45°C): At 45±3°C, charge the battery to 3.0V at a constant current of 0.33C, charge it to a cut-off current of 0.05C at a constant voltage of 3.0V, and then discharge it to 1.0V at a constant current of 1C. The discharge capacity is recorded as C1. Repeat the charge and discharge steps for 100 cycles to obtain the discharge capacity C1 at the Nth cycle. N , Nth cycle capacity retention rate = (C N / C1)×100%;

[0110] (5) Average Coulombic efficiency of the first 100 cycles (high temperature 45°C): Same as the test in step 2, the calculation method is as follows: Coulombic efficiency of each cycle CE = discharge capacity / charge capacity × 100%, average Coulombic efficiency of the first N cycles CE = SUM (CE1~CE N ) / N×100%;

[0111] (6) 3C / 0.5C capacity retention rate: At 25±3℃, charge at 0.5C constant current to 3.0V, charge at 3.0V constant voltage to a cut-off current of 0.05C, and then discharge the battery at 0.5C constant current to 1.0V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as A; charge at 0.5C constant current to 3.0V, charge at 3.0V constant voltage to a cut-off current of 0.05C, and then discharge the battery at 3C constant current to 1.0V; cycle for 5 times, record the discharge capacity of each cycle, and take the average as B. 3C / 0.5C capacity retention rate = B / A×100%.

[0112] The test results are shown in Table 2.

[0113] Table 2 Battery electrical performance test results

[0114]

[0115] According to Examples 1 to 15 and Comparative Examples 1 to 5, it can be seen that the battery prepared using the electrolyte provided by the present invention has relatively ideal performance in terms of battery first efficiency, conductivity, capacity retention rate and other performance. According to the comparison between Examples 1 to 11 and Examples 12 to 15, it can be seen that ester co-solvents, fluorine-containing compounds and additives have a certain improvement effect on the electrical performance and cycle performance of the battery; according to Example 1 and Comparative Examples 4 and 5, it can be seen that when the C / O molar ratio of the ether solvent and the dipole moment of the low polarity solvent meet the value range provided by the present invention, the final comprehensive performance of the battery can have a relatively good performance.

[0116] The above is a detailed introduction to an electrolyte and a lithium-sulfur battery provided in an embodiment of the present invention. The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the technical solutions and core ideas of the present invention. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrolyte, characterized in that: comprising a first lithium salt, a second lithium salt, a first solvent, a second solvent and an additive; wherein the first lithium salt and the second lithium salt are different substances; The first solvent is an ether compound, and the C / O molar ratio of the ether compound is ≥8; The dipole moment of the second solvent is 3.13-6.2; The molar ratio of the first lithium salt, the second lithium salt, the first solvent and the second solvent is 1:1-5:2.5-5:2.5-5; The additive includes a benzenethiol compound and a nitrate, wherein the molar ratio of the benzenethiol compound to the nitrate is 1:10-30; the mass percentage of the additive in the electrolyte is 2%-15%; The electrolyte further comprises an ester co-solvent; the molar ratio of the ester co-solvent to the first lithium salt is 0.25-1:1; The electrolyte further includes a fluorine-containing compound; the molar ratio of the fluorine-containing compound to the first lithium salt is 8-30:

1.

2. The electrolyte according to claim 1, characterized in that The first lithium salt and the second lithium salt include any two of lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonyl)imide and lithium hexafluorophosphate; and / or, The first solvent comprises one or more of isobutyl ether, butyl ether, ethyl butyl ether, amyl ether, n-hexyl ether, heptyl ether, dioctyl ether, tert-butyl ether, methyl butyl ether, sec-butyl ether, ethylene glycol dibutyl ether, isopentyl ether and isobutyl tert-butyl ether; and / or, The second solvent includes one or more of tetrahydropyran, 2-methyltetrahydrofuran, furan, 2-(tetrahydrofuran-3-yl)acetonitrile, tetrahydropyranone, 3-ketopyran, tetrahydropyran-2-ol, 4-aldehyde tetrahydropyran, tetrahydropyran-3-carbonitrile, tetrahydropyran-4,4-dicarbonitrile, 2H-benzopyran-3-carbonitrile, (tetrahydropyran-4-ylidene)acetonitrile, 2H-pyran-3(6H)-one and 2-tetrahydropyran-3-ylideneacetonitrile.

3. The electrolyte according to claim 1, characterized in that The ester co-solvent includes one or more of ethylene carbonate, vinylene carbonate, vinyl sulfite, difluoroethylene carbonate and fluoroethylene carbonate.

4. The electrolyte according to claim 1, characterized in that The fluorine-containing compound includes one or more of polyfluoro, flutir, desflurane, sevoflurane, perfluorocyclic ether, trifluoroacetonitrile ether, hexafluoroisopropyl methyl ether, methyl nonafluorobutyl ether, perfluoropropyl vinyl ether and eicosyl-15-crown-5-ether.

5. The electrolyte according to claim 1, characterized in that The benzenethiol compound includes one or more of benzenethiol, pentafluorobenzenethiol, 3-aminobenzenethiol, 4-nitrobenzenethiol, 3-ethylbenzenethiol, 2-isopropylbenzenethiol, 4-methylthiobenzenethiol, 2,6-difluorobenzenethiol, 2-trifluoromethylbenzenethiol, 5-fluoro-2-methylbenzenethiol, 4-(4-fluoro-phenoxy)-benzenethiol, 1,4-phenyldithiol, 1,4-benzenedimethanethiol and 1,2-benzenedithiol; and / or, The nitrate includes one or more of potassium nitrate, cesium nitrate, nickel nitrate, zinc nitrate, manganese nitrate, indium nitrate, rubidium nitrate, cesium nitrate, magnesium nitrate, chromium nitrate, copper nitrate, lithium nitrate and cobalt nitrate.

6. A lithium-sulfur battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte is the electrolyte according to any one of claims 1 to 5.