A high-efficiency low-temperature carbon monoxide removal catalyst and its preparation method

By loading graphene oxide and copper nitrate on titanium dioxide, and further loading manganese nitrate and cerium nitrate, nanoparticles agglomeration are inhibited and a high specific surface area structure is formed, the problems of large particle size and high conversion temperature of non-precious metal catalysts are solved, and high carbon monoxide is achieved Low temperature removal and sulfur resistance improvement.

CN118384896BActive Publication Date: 2024-11-05SHANDONG JIASHENG BONA ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410834608.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-11-13
Filing Date
2024-06-26
Publication Date
2024-11-05
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing non-precious metal catalysts are prone to agglomeration during the preparation process, resulting in large particle size, low catalytic performance, and high complete conversion temperature, resulting in high energy consumption and difficulty in effectively removing carbon monoxide.

Method used

By loading graphene oxide and copper nitrate onto titanium dioxide, a solvothermal reaction is carried out, and manganese nitrate and cerium nitrate are further loaded to inhibit the agglomeration of nanoparticles, forming a high specific surface area and active void structure, and reducing the ignition temperature.

Benefits of technology

It realizes the efficient low-temperature removal of carbon monoxide of the catalyst, low ignition temperature, low complete conversion temperature, excellent catalytic activity, and good sulfur resistance. It is suitable for the purification of fixed source flue gas such as steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118384896B_ABST
    Figure CN118384896B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and discloses a method for preparing a catalyst for the removal of carbon monoxide at low temperature with high efficiency, including: preparing pre-treated titanium dioxide; adding graphene oxide and copper nitrate to an ethanol aqueous solution and stirring evenly, adding dropwise to the pre-treated titanium dioxide, stirring at 60-80°C, centrifuging, filtering, washing to obtain loaded titanium dioxide; adding loaded titanium dioxide to a sodium hydroxide solution and mixing evenly, solvent thermal reaction, solid-liquid separation, washing solids, and then adding to water to obtain a doped titanium dioxide suspension; adding manganese nitrate and cerium nitrate to water and stirring evenly, dripping the doped titanium dioxide suspension under stirring conditions, stirring until precipitation, standing, solid-liquid separation, washing, drying, calcining at 500-600°C, granulating, and sieving. The present invention is used to realize the efficient catalytic oxidation removal of carbon monoxide in exhaust gas, and has a low ignition temperature and a low complete conversion temperature. It is suitable for the purification of fixed source flue gas such as steel, coking, and cement, and has a wide range of industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a high-efficiency low-temperature carbon monoxide removal catalyst and a preparation method thereof. Background Art

[0002] Carbon monoxide is a product of incomplete oxidation of carbon. Incomplete combustion of traditional fossil fuels such as coal, oil, and natural gas, as well as biomass fuels, is the main source of carbon monoxide. Carbon monoxide is one of the six basic controlled pollutants in my country's "Ambient Air Quality Standards". Its emission sources are extensive. Almost all combustion devices, including boilers, heating furnaces, sintering furnaces, coke ovens, etc., will produce carbon monoxide.

[0003] my country is a major steel producer, and its steel output has been ranked first in the world for many years. At present, steel enterprises are major emitters of carbon monoxide, mainly from sintering machine head flue gas, steelmaking primary flue gas, coke oven and dry quenching flue gas. As the country pays more and more attention to air pollution, carbon monoxide emissions have become a new focus of attention, and strict requirements have been put forward for its emission standards. Developing a low-temperature and efficient catalyst that can remove carbon monoxide is currently the simplest and most convenient method. Although the use of technical means such as sintering flue gas circulation, adding burners to the primary flue gas outlet of the converter, improving the gas combustion efficiency of the coke oven combustion chamber, and controlling the air volume of the dry quenching coke oven can reduce the amount of carbon monoxide produced, there is still inevitably a certain amount of residual carbon monoxide in the above flue gas, which still needs further purification to achieve the environmental protection goal of low carbon monoxide emissions.

[0004] Using appropriate catalysts to make carbon monoxide in flue gas undergo oxidation reaction and convert it into carbon dioxide is one of the recognized effective treatment methods, and its core lies in the selection and preparation method of catalysts. At present, carbon monoxide oxidation catalysts are mainly divided into two categories according to their catalytic active components: precious metals and non-precious metals. Precious metal catalysts are mostly loaded catalysts in which Pd, Pt, Au, Ag and multi-component precious metals are loaded on carriers such as cordierite and activated alumina, but precious metal catalysts are expensive, which limits their use. Non-precious metal catalysts refer to catalysts whose active components can be pure metals or alloys. Non-precious metal catalysts can be used alone or loaded on carriers, and have more ways of use. Non-precious metal catalysts have become the most valuable catalysts due to their convenient preparation process, excellent catalytic performance and recyclability.

[0005] However, non-precious metal nanoparticles are prone to agglomeration during the preparation process, resulting in the generation of non-precious metal particles with relatively large particle size, which has a great impact on the subsequent application of the material and reduces the catalytic performance of the non-precious metal. At the same time, its complete conversion temperature is high, generally above 200°C, resulting in high energy consumption of the device, which needs to be solved urgently. Summary of the invention

[0006] Based on the technical problems existing in the background technology, the present invention proposes a high-efficiency low-temperature carbon monoxide removal catalyst and a preparation method thereof.

[0007] A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0008] S1. Dispersing fumed titanium dioxide P25 powder into anhydrous ethanol, and adding glacial acetic acid and tetrabutyl titanate in sequence under stirring to obtain pretreated titanium dioxide;

[0009] S2, adding graphene oxide and copper nitrate to an ethanol aqueous solution and stirring evenly, adding dropwise to the pretreated titanium dioxide under stirring, stirring at 60-80° C. for 10-30 min, adjusting the pH value of the system to 11-12, continuing stirring, centrifuging, filtering, and washing to obtain loaded titanium dioxide;

[0010] S3, adding the loaded titanium dioxide to the sodium hydroxide solution and mixing evenly, performing a solvent thermal reaction at 150-160° C. for 48-56 hours, separating the solid from the liquid, washing the solid, and then adding the solid to water to obtain a doped titanium dioxide suspension;

[0011] S4. Add manganese nitrate and cerium nitrate into water and stir evenly. Add the doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 1-5 hours, separate the solid and liquid, wash the solid to neutrality, dry, roast at 500-600℃ for 5-10 hours, granulate, and sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0012] Preferably, in S1, the mass ratio of fumed titanium dioxide P25, anhydrous ethanol, glacial acetic acid, and tetrabutyl titanate is 1-5:40-100:2-3:5-10.

[0013] Preferably, in S2, the mass fraction of the ethanol aqueous solution is 40-60%, and the mass ratio of graphene oxide, copper nitrate, ethanol aqueous solution, and pretreated titanium dioxide is 1-3:0.1-1:20-50:50-110.

[0014] Preferably, in S2, a sodium hydroxide solution with a concentration of 0.5-1.2 mol / L is used to adjust the pH value of the system to 11-12.

[0015] Preferably, the graphene oxide is activated graphene oxide, specifically: 1-3 parts of graphene oxide and 0.1-1 parts of isocyanatepropyltrimethoxysilane are added to 10-20 parts of N,N-dimethylformamide by weight, stirred at a temperature of 100-110°C for 1-2h, centrifuged, washed with ethanol, and freeze-dried, the product and 0.1-1 parts of nano-titanium dioxide are added to a 30-60wt% ethanol solution, stirred at a temperature of 60-80°C for 1-2h, centrifuged, washed with deionized water, and freeze-dried to obtain activated graphene oxide.

[0016] By activating graphene oxide and grafting nano-titanium dioxide with the cooperation of isocyanatepropyltrimethoxysilane, not only can the problem of easy agglomeration of graphene oxide be effectively solved, but also because the activated graphene oxide has amphiphilic properties, it can effectively enhance the dispersion uniformity of copper nitrate in doped titanium dioxide. In addition, the binding stability of graphene oxide in doped titanium dioxide is higher, and the catalytic activity is good after calcination.

[0017] Preferably, in S2, after filtering, the mixture is washed with anhydrous ethanol for 1-3 times.

[0018] Preferably, in S3, the concentration of the sodium hydroxide solution is 9-12 mol / L, and the mass ratio of the loaded titanium dioxide, the sodium hydroxide solution, and water is 9-22:20-30:20-30.

[0019] Preferably, in S3, the solid matter is washed with deionized water until the pH value is 10.5-11.2.

[0020] Preferably, in S4, the mass ratio of manganese nitrate, cerium nitrate, water, and doped titanium dioxide suspension is 1-2:0.1-1:40-100:30-50.

[0021] Preferably, in S4, the drying temperature is 100-120°C.

[0022] A high-efficiency carbon monoxide low-temperature removal catalyst is prepared by adopting the high-efficiency carbon monoxide low-temperature removal catalyst preparation method. Beneficial Effects

[0023] In the present invention, graphene oxide and copper nitrate are loaded onto titanium dioxide, copper ions are doped into the titanium dioxide structure through a solvent thermal reaction, and manganese nitrate and cerium nitrate are further loaded, so that non-precious metal nanoparticles of copper, manganese and cerium are loaded in sequence, the agglomeration growth of non-precious metal nanoparticles is inhibited, and the particle size of the nanoparticles is reduced. The graphene oxide therein is removed through calcination to form a large number of active void structures, which effectively increases the specific surface area of ​​the catalyst and has high catalytic activity. At the same time, the applicant has found that the present invention can greatly reduce the ignition temperature on the basis of greatly improving the catalytic oxidation performance of the catalyst for carbon monoxide, and has an excellent catalytic effect.

[0024] The present invention not only has high structural stability, but also has a very large specific surface area, high pore volume, high mesopore order, high catalytic activity, and excellent sulfur resistance. It has good catalytic performance for catalytic oxidation and removal of carbon monoxide from flue gas containing sulfur dioxide.

[0025] The present invention is used to realize the efficient catalytic oxidation removal of carbon monoxide in the exhaust gas, and has a low ignition temperature and a low complete conversion temperature. -1 Under the conditions of , the ignition temperature can be lower than 112 ℃, and the complete conversion of carbon monoxide can be achieved at 145 ℃. It is suitable for the purification of flue gas from fixed sources such as steel, coking, cement, etc., and has a wide range of industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The N2 adsorption-desorption isotherms of the catalysts obtained in Example 5 and Comparative Examples 1-2 are shown.

[0027] Figure 2 The pore size distribution diagram of the catalysts obtained in Example 5 and Comparative Examples 1-2.

[0028] Figure 3 This is a comparison chart of the carbon monoxide conversion rate and sulfur dioxide conversion rate of the catalyst obtained in Example 5.

[0029] Figure 4 It is a comparison chart of the ignition temperature, complete conversion temperature and carbon monoxide conversion rate of the catalysts obtained in Examples 5-6 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is described in detail below through specific embodiments.

[0031] Example 1 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0032] S1. Disperse 1 g of fumed titanium dioxide P25 powder into 40 g of anhydrous ethanol, add 2 g of glacial acetic acid and 5 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 500 r / min for 1 h to obtain pretreated titanium dioxide;

[0033] S2. Add 1g of graphene oxide and 0.1g of copper nitrate to 20g of 40% ethanol aqueous solution and stir evenly. Add dropwise to 50g of pretreated titanium dioxide under stirring at a speed of 50r / min. Stir at 60°C for 10min. Use 0.5mol / L sodium hydroxide solution to adjust the pH value of the system to 11-12. Stir at a speed of 100r / min for 5min. Centrifuge, filter, and wash once with anhydrous ethanol to obtain loaded titanium dioxide.

[0034] S3, 9g of loaded titanium dioxide was added to 20g of 9mol / L sodium hydroxide solution and mixed evenly, and then sent to a hydrothermal reactor lined with polytetrafluoroethylene, and placed at a temperature of 150°C for 48h for solid-liquid separation. The solid was washed with deionized water until the pH value was 10.5-11.2, and then added to 20g of water to prepare a doped titanium dioxide suspension;

[0035] S4. Add 1g of manganese nitrate and 0.1g of cerium nitrate to 40g of water and stir evenly. Add 30g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 1h, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 100°C, calcine in a muffle furnace at 500°C for 5h, granulate, and pass through a 40-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0036] Example 2 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0037] S1. Disperse 5 g of fumed titanium dioxide P25 powder into 100 g of anhydrous ethanol, add 3 g of glacial acetic acid and 10 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1500 r / min for 2 h to obtain pretreated titanium dioxide;

[0038] S2, add 3g of graphene oxide and 1g of copper nitrate to 50g of 60% ethanol aqueous solution and stir evenly, add dropwise to 110g of pretreated titanium dioxide under stirring, stirring at a speed of 100r / min, stirring at a temperature of 80°C for 30min, using a 1.2mol / L sodium hydroxide solution to adjust the pH value of the system to 11-12, stirring at a speed of 500r / min for 20min, centrifuging, filtering, and washing 3 times with anhydrous ethanol to obtain loaded titanium dioxide;

[0039] S3, add 22g of loaded titanium dioxide to 30g of 12mol / L sodium hydroxide solution and mix well, send it into a hydrothermal reactor lined with polytetrafluoroethylene, place it at a temperature of 160°C for 56h, separate the solid and liquid, wash the solid with deionized water to a pH value of 10.5-11.2, and add it to 30g of water to prepare a doped titanium dioxide suspension;

[0040] S4. Add 2g of manganese nitrate and 1g of cerium nitrate to 100g of water and stir evenly. Add 50g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 5h, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 120°C, calcine at 600°C in a muffle furnace for 10h, granulate, and pass through a 60-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0041] Example 3 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0042] S1. Disperse 2 g of fumed titanium dioxide P25 powder into 80 g of anhydrous ethanol, add 2.2 g of glacial acetic acid and 9 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 800 r / min for 100 min to obtain pretreated titanium dioxide;

[0043] S2, 1.5g of graphene oxide and 0.7g of copper nitrate were added to 30g of 55% ethanol aqueous solution and stirred evenly, and then added dropwise to 70g of pretreated titanium dioxide under stirring, with a stirring speed of 90r / min, stirred at a temperature of 65°C for 25min, and the pH value of the system was adjusted to 11-12 with a concentration of 0.8mol / L sodium hydroxide solution, stirred at a speed of 400r / min for 10min, centrifuged, filtered, and washed twice with anhydrous ethanol to obtain loaded titanium dioxide;

[0044] S3, 18g of loaded titanium dioxide was added to 22g of 11mol / L sodium hydroxide solution and mixed evenly, and sent to a hydrothermal reactor lined with polytetrafluoroethylene, and placed at a temperature of 152°C for 54h, solid-liquid separation, the solid was washed with deionized water to a pH value of 10.5-11.2, and added to 22g of water to prepare a doped titanium dioxide suspension;

[0045] S4. Add 1.7 g of manganese nitrate and 0.3 g of cerium nitrate into 80 g of water and stir evenly. Add 35 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 4 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 105°C, calcine in a muffle furnace at 580°C for 7 hours, granulate, and pass through a 55-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0046] Example 4 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0047] S1. Disperse 4 g of fumed titanium dioxide P25 powder into 60 g of anhydrous ethanol, add 2.8 g of glacial acetic acid and 7 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1200 r / min for 80 min to obtain pretreated titanium dioxide;

[0048] S2, add 2.5g of graphene oxide and 0.3g of copper nitrate to 40g of 45% ethanol aqueous solution and stir evenly, add dropwise to 90g of pretreated titanium dioxide under stirring, stirring speed is 70r / min, stir at temperature 75°C for 15min, adjust the pH value of the system to 11-12 with 1mol / L sodium hydroxide solution, stir at 200r / min for 16min, centrifuge, filter, wash twice with anhydrous ethanol, and obtain loaded titanium dioxide;

[0049] S3, 14g of loaded titanium dioxide was added to 28g of 10mol / L sodium hydroxide solution and mixed evenly, and sent to a hydrothermal reactor lined with polytetrafluoroethylene, and placed at a temperature of 158°C for 50h, solid-liquid separation, and the solid was washed with deionized water to a pH value of 10.5-11.2, and added to 28g of water to prepare a doped titanium dioxide suspension;

[0050] S4. Add 1.3 g of manganese nitrate and 0.7 g of cerium nitrate into 60 g of water and stir evenly. Add 45 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 2 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 115°C, calcine in a muffle furnace at 520°C for 9 hours, granulate, and pass through a 45-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0051] Example 5 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0052] S1. Disperse 3 g of fumed titanium dioxide P25 powder into 70 g of anhydrous ethanol, add 2.5 g of glacial acetic acid and 8 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1000 r / min for 90 min to obtain pretreated titanium dioxide;

[0053] S2, add 2g of graphene oxide and 0.5g of copper nitrate to 35g of 50% ethanol aqueous solution and stir evenly, add dropwise to 80g of pretreated titanium dioxide under stirring, stirring speed is 80r / min, stir at temperature 70°C for 20min, adjust the pH value of the system to 11-12 with 0.9mol / L sodium hydroxide solution, stir at 300r / min for 13min, centrifuge, filter, wash twice with anhydrous ethanol, and obtain loaded titanium dioxide;

[0054] S3, add 16g of loaded titanium dioxide to 25g of 10.5mol / L sodium hydroxide solution and mix well, send it into a hydrothermal reactor lined with polytetrafluoroethylene, place it at a temperature of 155°C for 52h, separate the solid and liquid, wash the solid with deionized water to a pH value of 10.5-11.2, and add it to 25g of water to prepare a doped titanium dioxide suspension;

[0055] S4. Add 1.5 g of manganese nitrate and 0.5 g of cerium nitrate into 70 g of water and stir evenly. Add 40 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 3 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 110°C, calcine in a muffle furnace at 550°C for 8 hours, granulate, and pass through a 50-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0056] Comparative Example 1

[0057] A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0058] S1. Disperse 3 g of fumed titanium dioxide P25 powder into 70 g of anhydrous ethanol, add 2.5 g of glacial acetic acid and 8 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1000 r / min for 90 min to obtain pretreated titanium dioxide;

[0059] S2, add 0.5g copper nitrate to 35g of 50% ethanol aqueous solution and stir evenly, add dropwise to 80g pretreated titanium dioxide under stirring, stirring speed is 80r / min, stir at temperature 70°C for 20min, adjust the pH value of the system to 11-12 with 0.9mol / L sodium hydroxide solution, stir at 300r / min for 13min, centrifuge, filter, wash twice with anhydrous ethanol, and obtain loaded titanium dioxide;

[0060] S3, add 16g of loaded titanium dioxide to 25g of 10.5mol / L sodium hydroxide solution and mix well, send it into a hydrothermal reactor lined with polytetrafluoroethylene, place it at a temperature of 155°C for 52h, separate the solid and liquid, wash the solid with deionized water to a pH value of 10.5-11.2, and add it to 25g of water to prepare a doped titanium dioxide suspension;

[0061] S4. Add 1.5 g of manganese nitrate and 0.5 g of cerium nitrate into 70 g of water and stir evenly. Add 40 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 3 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 110°C, calcine in a muffle furnace at 550°C for 8 hours, granulate, and pass through a 50-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0062] Comparative Example 2

[0063] A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0064] S1. Disperse 3 g of fumed titanium dioxide P25 powder into 70 g of anhydrous ethanol, add 2.5 g of glacial acetic acid and 8 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1000 r / min for 90 min to obtain pretreated titanium dioxide;

[0065] S2, adding 2g of graphene oxide to 35g of 50% ethanol aqueous solution and stirring evenly, adding dropwise to 80g of pretreated titanium dioxide under stirring, stirring at a speed of 80r / min, stirring at a temperature of 70°C for 20min, adjusting the pH value of the system to 11-12 with a concentration of 0.9mol / L sodium hydroxide solution, stirring at a speed of 300r / min for 13min, centrifuging, filtering, and washing twice with anhydrous ethanol to obtain loaded titanium dioxide;

[0066] S3, add 16g of loaded titanium dioxide to 25g of 10.5mol / L sodium hydroxide solution and mix well, send it into a hydrothermal reactor lined with polytetrafluoroethylene, place it at a temperature of 155°C for 52h, separate the solid and liquid, wash the solid with deionized water to a pH value of 10.5-11.2, and add it to 25g of water to prepare a doped titanium dioxide suspension;

[0067] S4. Add 1.5 g of manganese nitrate, 0.5 g of cerium nitrate and 0.5 g of copper nitrate into 70 g of water and stir evenly. Add 40 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 3 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 110°C, calcine in a muffle furnace at 550°C for 8 hours, granulate, and pass through a 50-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0068] The catalysts obtained in Example 5 and Comparative Examples 1-2 were subjected to N2 adsorption-desorption isotherm analysis (BET): the samples were degassed at 200°C for 4 h before testing, the specific surface area was calculated using the BET method, and the pore size and pore volume were calculated using the BJH method.

[0069] like Figure 1 and Figure 2 As shown, the catalysts obtained in Example 5 and Comparative Examples 1-2 all exhibit type IV adsorption isotherms, indicating that all three have mesoporous structures, but the catalyst obtained in Example 5 has a larger specific surface area and pore size, making it easier to absorb carbon monoxide for oxidation treatment.

[0070] The catalyst obtained in Example 5 was tested for its water and sulfur resistance: 0.1 g of each sample was placed in a fixed bed quartz tube reactor (quartz tube inner diameter = 6 mm), and the simulated flue gas consisted of CO, SO2, water vapor, O2 and N2, wherein the carbon monoxide concentration was 10000 ppm, the SO2 concentration was 300 ppm, the water vapor volume fraction was 10%, the O2 volume fraction was 10%, and the rest was N2, and the air velocity was 30000 h -1 , the temperature was maintained at 150°C, and other test conditions remained unchanged.

[0071] like Figure 3 As shown, it is proved that the catalyst obtained in Example 5 has strong resistance to water and sulfur.

[0072] Example 6 A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst comprises the following steps:

[0073] S1. Disperse 3 g of fumed titanium dioxide P25 powder into 70 g of anhydrous ethanol, add 2.5 g of glacial acetic acid and 8 g of tetrabutyl titanate in sequence under stirring, and stir at a speed of 1000 r / min for 90 min to obtain pretreated titanium dioxide;

[0074] S2, adding 2g of graphene oxide and 0.2g of isocyanatepropyltrimethoxysilane to 12g of N,N-dimethylformamide, stirring at 106°C for 1.5h, centrifuging, washing with ethanol, freeze-drying, adding the product and 0.2g of nano-titanium dioxide to 10-20 parts of 45wt% ethanol solution, stirring at 70°C for 1h, centrifuging, washing with deionized water, freeze-drying, and obtaining activated graphene oxide;

[0075] Add activated graphene oxide and 0.5g copper nitrate to 35g of 50% ethanol aqueous solution and stir evenly, then add dropwise to 80g pretreated titanium dioxide under stirring, at a stirring speed of 80r / min, stir at a temperature of 70°C for 20min, adjust the pH value of the system to 11-12 with a 0.9mol / L sodium hydroxide solution, stir at a speed of 300r / min for 13min, centrifuge, filter, and wash twice with anhydrous ethanol to obtain loaded titanium dioxide;

[0076] S3, add 16g of loaded titanium dioxide to 25g of 10.5mol / L sodium hydroxide solution and mix well, send it into a hydrothermal reactor lined with polytetrafluoroethylene, place it at a temperature of 155°C for 52h, separate the solid and liquid, wash the solid with deionized water to a pH value of 10.5-11.2, and add it to 25g of water to prepare a doped titanium dioxide suspension;

[0077] S4. Add 1.5 g of manganese nitrate and 0.5 g of cerium nitrate into 70 g of water and stir evenly. Add 40 g of doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 3 hours, separate the solid and liquid, wash the solid with deionized water until it is neutral, dry at 110°C, calcine in a muffle furnace at 550°C for 8 hours, granulate, and pass through a 50-mesh sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

[0078] The catalyst activity test was carried out on the catalysts obtained in Examples 5-6 and Comparative Examples 1-2: 0.1 g of each sample was placed in a fixed bed quartz tube reactor (quartz tube inner diameter = 6 mm), and the simulated flue gas consisted of CO, O2 and N2, wherein the carbon monoxide concentration was 10000 ppm, the O2 volume fraction was 10%, the N2 volume fraction was 89%, and the air velocity was 30000 h -1 , the reaction temperature is 100-200℃.

[0079] The results are as follows Figure 4 As shown, the ignition temperature and complete conversion temperature of the catalysts obtained in Example 5 and Example 6 are lower than those in Comparative Example 1-2 (P < 0.05), while the carbon monoxide conversion rate is higher than that in Comparative Example 1-2 (P < 0.05).

[0080] At the same time, the carbon monoxide conversion rates of the catalysts obtained in Example 5 and Example 6 were both over 99%, with no significant difference between the two (P>0.05), but the ignition temperature and complete conversion temperature of the catalyst obtained in Example 6 were lower than those in Example 5 (P<0.05).

[0081] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst, characterized in that: The steps include: S1. Dispersing fumed titanium dioxide P25 powder into anhydrous ethanol, and adding glacial acetic acid and tetrabutyl titanate in sequence under stirring to obtain pretreated titanium dioxide; S2, adding graphene oxide and copper nitrate to an ethanol aqueous solution and stirring evenly, adding dropwise to the pretreated titanium dioxide under stirring, stirring at 60-80° C. for 10-30 min, adjusting the pH value of the system to 11-12, continuing stirring, centrifuging, filtering, and washing to obtain loaded titanium dioxide; The mass fraction of the ethanol aqueous solution is 40-60%, and the mass ratio of graphene oxide, copper nitrate, ethanol aqueous solution, and pretreated titanium dioxide is 1-3: 0.1-1: 20-50: 50-110; S3, adding the loaded titanium dioxide to the sodium hydroxide solution and mixing evenly, performing a solvent thermal reaction at 150-160° C. for 48-56 hours, separating the solid from the liquid, washing the solid, and then adding the solid to water to obtain a doped titanium dioxide suspension; The concentration of the sodium hydroxide solution is 9-12 mol / L, and the mass ratio of the loaded titanium dioxide, the sodium hydroxide solution, and water is 9-22:20-30:20-30; S4. Add manganese nitrate and cerium nitrate into water and stir evenly. Add the doped titanium dioxide suspension dropwise under stirring, stir until the precipitation is complete, let stand for 1-5 hours, separate the solid and liquid, wash the solid to neutrality, dry, roast at 500-600℃ for 5-10 hours, granulate, and sieve to obtain a high-efficiency low-temperature carbon monoxide removal catalyst.

2. The method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to claim 1, characterized in that: In S1, the mass ratio of fumed titanium dioxide P25, anhydrous ethanol, glacial acetic acid, and tetrabutyl titanate is 1-5:40-100:2-3:5-10.

3. The method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to claim 1, characterized in that: In S2, a sodium hydroxide solution with a concentration of 0.5-1.2 mol / L is used to adjust the pH value of the system to 11-12.

4. The method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to claim 1, characterized in that: In S3, the solid matter is washed with deionized water until the pH value is 10.5-11.

2.

5. The method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to claim 1, characterized in that: In S4, the mass ratio of manganese nitrate, cerium nitrate, water, and doped titanium dioxide suspension is 1-2:0.1-1:40-100:30-50.

6. The method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to claim 1, characterized in that: In S4, the drying temperature is 100-120°C.

7. A high-efficiency low-temperature carbon monoxide removal catalyst, characterized in that: The catalyst is prepared by the method for preparing a high-efficiency low-temperature carbon monoxide removal catalyst according to any one of claims 1 to 6.