A concrete composite admixture and preparation method thereof

By using composite admixtures composed of tetrahydroxymethylglycoloururide in concrete, combined with nano zinc oxide and fly ash fiber and other materials, the insufficient compressive strength, impermeability and crack resistance and durability of concrete in the prior art are solved. The problem of this paper achieves the effect of low usage and high efficiency, and improves the comprehensive performance and stability of building materials.

CN118388168BActive Publication Date: 2024-11-22NINGBO XINLI CEMENT PROD CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202311071992.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-24
Publication Date
2024-11-22
Estimated Expiration
2043-08-24

AI Technical Summary

Technical Problem

The existing concrete composite admixtures still have room for improvement in improving the compressive strength, seepage and crack resistance and durability of concrete, and the use volume is large and the performance stability is insufficient, which affects the quality of construction projects.

Method used

Using tetrahydroxymethylglycoloured urea, piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), water-soluble polymeric cyclodextrin, hyperbranched polyglycerol, nano zinc oxide, fly ash fiber, 1- A concrete composite admixture composed of benzylpyridine-3-carboxylate and functional copolymer is prepared by free radical copolymerization, and combined with ball mill grinding technology to improve the compatibility and dispersion of components.

Benefits of technology

It significantly improves the compressive strength, seepage and crack resistance and durability of concrete, reduces the amount of use, enhances compactness, resists harmful ions intrusion, improves comprehensive performance and performance stability, and is suitable for high-performance concrete needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a concrete composite admixture and a preparation method thereof, and relates to the technical field of building materials, comprising the following components by weight: 1-3 parts of tetramethylol glycoluril, 2-4 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1-3 parts of water-soluble polymerized cyclodextrin, 3-5 parts of hyperbranched polyglycerol, 1-3 parts of nano zinc oxide, 1-3 parts of fly ash fiber, 0.8-1.5 parts of 1-benzylpyridine-3-carboxylate, 1-4 parts of surfactant, and 1-2 parts of functional copolymer. The admixture has a small dosage, good comprehensive efficiency, and small negative impact on concrete, and can effectively improve the compressive strength, anti-seepage and anti-cracking performance and durability of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a concrete composite admixture and a preparation method thereof. Background Art

[0002] Concrete is the main material of modern construction projects. It is an artificial stone made of cementitious materials, granular aggregates (also called aggregates), water, and admixtures in a certain proportion, which are uniformly mixed, compacted, and hardened. The quality of concrete directly determines the quality of construction projects, and the use of concrete admixtures is indispensable for concrete to exert its excellent performance. Adding concrete admixtures has become the main measure to improve the performance of concrete.

[0003] There are a wide variety of concrete admixtures on the market, such as waterproofing agents, antifreeze agents, quick setting agents, retarder agents, early strength agents, water reducing agents, etc. These admixtures can play their own single functions. However, to improve the comprehensive performance of concrete, it is often necessary to add a variety of different types of admixtures to it at the same time. Concrete admixtures with single functions are increasingly unsuitable for the development of high-performance concrete technology. It is under this situation that concrete composite admixtures came into being, and its appearance has attracted widespread attention.

[0004] Concrete composite admixtures are admixtures with more than two main functions. The use of composite admixtures can not only effectively optimize the performance of concrete, but also reduce the production cost of concrete, realize the comprehensive utilization of industrial waste, and reduce environmental pollution. However, the concrete composite admixtures on the market still have more or less technical defects such as large addition amount, the comprehensive performance and performance stability need to be further improved, and there is a negative impact on the performance of concrete.

[0005] In order to solve the above problems, Chinese invention patent document 201110100219.5 discloses a concrete composite admixture, whose composition and proportion are respectively: high-efficiency water reducing agent 17.5-58.0wt%, silicone waterproofing agent 0.5-5.5wt%, silicone reinforcing agent 0.2-2.5wt%, polyacrylamide 3.5-25wt%, triethanolamine 1.2-2.8wt%, sodium nitrite 3.2-6.3wt%, ethylene glycol 0.3-1.2wt%, glycerol 0.6-1.3wt%, sodium gluconate 2.8-5.5wt% and the balance of water. The composite admixture of the application can significantly improve the impact resistance, friction resistance and anti-seepage and waterproof performance of the concrete material in the process of concrete configuration, so it is particularly suitable for the requirements of high-performance concrete for airport runways or highway bridge construction. However, the compressive strength, anti-seepage and anti-cracking performance and durability of the concrete using the composite admixture still need to be further improved.

[0006] It can be seen that the art still needs a concrete composite admixture and a preparation method thereof that has a small dosage, good comprehensive performance, small negative impact on concrete, and can effectively improve the compressive strength, impermeability, crack resistance and durability of concrete. Summary of the invention

[0007] The main purpose of the present invention is to provide a concrete composite admixture and a preparation method thereof which has small dosage, good comprehensive efficiency, small negative impact on concrete, and can effectively improve the compressive strength, impermeability, crack resistance and durability of concrete.

[0008] To achieve the above purpose, the present invention provides a concrete composite admixture, comprising the following components in parts by weight: 1-3 parts of tetrakishydroxymethyl glycoluril, 2-4 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1-3 parts of water-soluble polymerized cyclodextrin, 3-5 parts of hyperbranched polyglycerol, 1-3 parts of nano zinc oxide, 1-3 parts of fly ash fiber, 0.8-1.5 parts of 1-benzylpyridine-3-carboxylate, 1-4 parts of surfactant, and 1-2 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0009] Preferably, the preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator to a high boiling point solvent, stirring and reacting at 50-65° C. in an inert gas atmosphere for 4-6 hours, then removing the solvent by rotary evaporation, washing with ethanol 3-6 times, and then drying in a vacuum drying oven at 85-95° C. to constant weight to obtain a functional copolymer.

[0010] Preferably, the mass ratio of the 2-acrylamido-2-methylpropanesulfonic acid, 2-vinylpyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator, and high boiling point solvent is 3:(1-2):1:(0.8-1.3):(0.06-0.1):(20-30).

[0011] Preferably, the initiator is azobisisobutyronitrile; the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone; and the inert gas is any one of nitrogen, helium, neon, and argon.

[0012] Preferably, the surfactant is one or more of fatty alcohol polyoxyethylene ether, nonylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether phosphate.

[0013] Preferably, the fly ash fiber has a diameter of 1 to 10 μm and can be prepared using the technology disclosed in Patent ZL200410018352.6.

[0014] Preferably, the particle size of the nano zinc oxide is 20-80 nm.

[0015] Preferably, there is no special requirement for the source of the hyperbranched polyglycerol. In one embodiment of the present invention, the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8.

[0016] Preferably, the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0017] Another object of the present invention is to provide a method for preparing the concrete composite admixture, comprising the following steps: mixing the components uniformly by weight, adding the components into a ball mill, grinding for 10-20 minutes, and then discharging the components to obtain the concrete composite admixture.

[0018] Due to the application of the above technical solution, the present invention has the following beneficial effects:

[0019] (1) The preparation method of the concrete composite admixture disclosed in the present invention only requires mixing the components in parts by weight uniformly. The operation is convenient and easy, no special equipment and production line are required, energy consumption is low, preparation efficiency and finished product qualification rate are high, and the method is suitable for industrial production.

[0020] (2) The concrete composite admixture disclosed in the present invention comprises the following components in parts by weight: 1-3 parts of tetrakishydroxymethyl glycoluril, 2-4 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1-3 parts of water-soluble polymerized cyclodextrin, 3-5 parts of hyperbranched polyglycerol, 1-3 parts of nano zinc oxide, 1-3 parts of fly ash fiber, 0.8-1.5 parts of 1-benzylpyridine-3-carboxylate, 1-4 parts of surfactant, and 1-2 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate. Through the mutual coordination between the components, the prepared concrete composite admixture has a small dosage, good comprehensive performance, and small negative impact on concrete. It can effectively improve the compressive strength, anti-seepage and crack resistance and durability of concrete.

[0021] (3) The concrete composite admixture disclosed in the present invention, through the addition of nano zinc oxide and fly ash fibers, cooperates with other components, so that it can improve the compactness, anti-seepage and anti-cracking capabilities, and effectively resist the ability of harmful ions such as chloride ions and sulfate ions to enter the interior of the concrete, thereby significantly improving the durability of the concrete. Through the reasonable selection of tetrahydroxymethyl glycoluril, piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), water-soluble polymerized cyclodextrin, and hyperbranched polyglycerol, they can better interact with each other, and can simultaneously play the role of water reduction, air entrainment, antifreeze, and slow setting, effectively improving the strength of the concrete and resolving the destructive effects of the external environment on the concrete structure; at the same time, these structures can also improve the compatibility and dispersibility between the components, thereby further improving the comprehensive performance and performance stability of the concrete using the composite admixture.

[0022] (4) The concrete composite admixture disclosed in the present invention, the addition of 1-benzylpyridine-3-carboxylate amphoteric organic salt can promote the formation of calcium silicate hydrate, improve the pore structure of the hydration product, and enhance the compactness of the concrete structure; in addition, it can also improve the compatibility and dispersibility between the components, thereby improving the compressive strength, impermeability, crack resistance and durability of the concrete using the product.

[0023] (5) The concrete composite admixture disclosed in the present invention is added with a functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate; sulfonate, pyrimidine, benzotriazole and diphenylpentane structures are simultaneously introduced into the molecular structure of the copolymer, and these structures can improve the water-reducing performance and the durability of the concrete using the composite admixture under the multiple effects of electronic effect, steric effect and conjugation effect. DETAILED DESCRIPTION

[0024] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1

[0025] A concrete composite admixture comprises the following components in parts by weight: 1 part of tetrakishydroxymethyl glycoluril, 2 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1 part of water-soluble polymerized cyclodextrin, 3 parts of hyperbranched polyglycerol, 1 part of nano zinc oxide, 1 part of fly ash fiber, 0.8 parts of 1-benzylpyridine-3-carboxylate, 1 part of surfactant, and 1 part of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0026] The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator into a high boiling point solvent, stirring and reacting at 50°C for 4 hours in an inert gas atmosphere, then removing the solvent by rotary evaporation, washing with ethanol for 3 times, and then drying in a vacuum drying oven at 85°C. The mixture is dried to constant weight to obtain a functional copolymer; the mass ratio of the 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator, and high boiling point solvent is 3:1:1:0.8:0.06:20; the initiator is azobisisobutyronitrile; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.

[0027] The surfactant is fatty alcohol polyoxyethylene ether; the diameter of the fly ash fiber is 1 μm, which can be prepared using the technology disclosed in patent ZL200410018352.6; the particle size of the nano zinc oxide is 20 nm; the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8; the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0028] A preparation method of the concrete composite admixture comprises the following steps: after uniformly mixing the components by weight, adding the components into a ball mill and grinding for 10 minutes, discharging the components to obtain the concrete composite admixture. Example 2

[0029] A concrete composite admixture comprises the following components in parts by weight: 1.5 parts of tetrakishydroxymethyl glycoluril, 2.5 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1.5 parts of water-soluble polymerized cyclodextrin, 3.5 parts of hyperbranched polyglycerol, 1.5 parts of nano zinc oxide, 1.5 parts of fly ash fiber, 1 part of 1-benzylpyridine-3-carboxylate, 2 parts of surfactant, and 1.2 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0030] The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamide-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate and an initiator to a high boiling point solvent, stirring and reacting at 55° C. for 4.5 hours in an inert gas atmosphere, then removing the solvent by rotary evaporation, washing with ethanol for 4 times, and then drying to constant weight in a vacuum drying oven at 87° C. to obtain the functional copolymer; the mass ratio of the 2-acrylamide-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, the initiator and the high boiling point solvent is 3:1.2:1: 0.9:0.07:22; the initiator is azobisisobutyronitrile; the high boiling point solvent is N,N-dimethylformamide; and the inert gas is helium.

[0031] The surfactant is nonylphenol polyoxyethylene ether; the diameter of the fly ash fiber is 3 μm, which can be prepared using the technology disclosed in patent ZL200410018352.6; the particle size of the nano zinc oxide is 30 nm; the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8; the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0032] A preparation method of the concrete composite admixture comprises the following steps: after uniformly mixing the components by weight, adding the components into a ball mill and grinding for 12 minutes, discharging the components to obtain the concrete composite admixture. Example 3

[0033] A concrete composite admixture comprises the following components in parts by weight: 2 parts of tetrakishydroxymethyl glycoluril, 3 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 2 parts of water-soluble polymerized cyclodextrin, 4 parts of hyperbranched polyglycerol, 2 parts of nano zinc oxide, 2 parts of fly ash fiber, 1.2 parts of 1-benzylpyridine-3-carboxylate, 2.5 parts of surfactant, and 1.5 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0034] The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator into a high boiling point solvent, stirring and reacting at 59° C. for 5 hours in an inert gas atmosphere, then removing the solvent by rotary evaporation, washing with ethanol for 5 times, and then drying in a vacuum drying oven at 90° C. to a constant temperature. The weight ratio of 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator and high boiling point solvent is 3:1.5:1:1.1:0.08:25; the initiator is azobisisobutyronitrile; the high boiling point solvent is N-methylpyrrolidone; and the inert gas is neon.

[0035] The surfactant is fatty alcohol polyoxyethylene ether phosphate; the diameter of the fly ash fiber is 6 μm, which can be prepared using the technology disclosed in patent ZL200410018352.6; the particle size of the nano zinc oxide is 50 nm; the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8; the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0036] A preparation method of the concrete composite admixture comprises the following steps: after uniformly mixing the components by weight, adding the components into a ball mill and grinding for 15 minutes, discharging the components to obtain the concrete composite admixture. Example 4

[0037] A concrete composite admixture comprises the following components in parts by weight: 2.5 parts of tetrakishydroxymethyl glycoluril, 3.5 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 2.5 parts of water-soluble polymerized cyclodextrin, 4.5 parts of hyperbranched polyglycerol, 2.5 parts of nano zinc oxide, 2.5 parts of fly ash fiber, 1.4 parts of 1-benzylpyridine-3-carboxylate, 3.5 parts of surfactant, and 1.8 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0038] The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator to a high boiling point solvent, stirring and reacting at 63° C. in an inert gas atmosphere for 5.5 hours, then removing the solvent by rotary evaporation, washing with ethanol for 6 times, and then drying in a vacuum drying oven at 93° C. to constant weight to obtain the functional copolymer; the 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator are added to a high boiling point solvent, and reacting at 63° C. in an inert gas atmosphere for 5.5 hours, then removing the solvent by rotary evaporation, washing with ethanol for 6 times, and then drying in a vacuum drying oven at 93° C. to constant weight to obtain the functional copolymer; The mass ratio of enamido-2-methylpropanesulfonic acid, 2-vinylpyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator, and high boiling point solvent is 3:1.8:1:1.2:0.09:28; the initiator is azobisisobutyronitrile; the high boiling point solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone in a mass ratio of 1:3:5; and the inert gas is argon.

[0039] The surfactant is a mixture of fatty alcohol polyoxyethylene ether, nonylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether phosphate in a mass ratio of 1:2:3; the diameter of the fly ash fiber is 9 μm, and can be prepared using the technology disclosed in patent ZL200410018352.6; the particle size of the nano zinc oxide is 70 nm; the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8; the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0040] A preparation method of the concrete composite admixture comprises the following steps: after uniformly mixing the components by weight, adding the components into a ball mill and grinding for 18 minutes, discharging the components to obtain the concrete composite admixture. Example 5

[0041] A concrete composite admixture comprises the following components in parts by weight: 3 parts of tetrakishydroxymethyl glycoluril, 4 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 3 parts of water-soluble polymerized cyclodextrin, 5 parts of hyperbranched polyglycerol, 3 parts of nano zinc oxide, 3 parts of fly ash fiber, 1.5 parts of 1-benzylpyridine-3-carboxylate, 4 parts of surfactant, and 2 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate.

[0042] The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator into a high boiling point solvent, stirring and reacting at 65° C. for 6 hours in an inert gas atmosphere, then removing the solvent by rotary evaporation, washing with ethanol for 6 times, and then placing in a vacuum drying oven at 95° C. Dry to constant weight to obtain a functional copolymer; the mass ratio of the 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator, and high boiling point solvent is 3:2:1:1.3:0.1:30; the initiator is azobisisobutyronitrile; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.

[0043] The surfactant is fatty alcohol polyoxyethylene ether; the diameter of the fly ash fiber is 10 μm, which can be prepared using the technology disclosed in patent ZL200410018352.6; the particle size of the nano zinc oxide is 80 nm; the hyperbranched polyglycerol is prepared according to the method of Example 1 in Chinese invention patent document CN202111038640.8; the CAS number of the water-soluble polymerized cyclodextrin is 25655-42-9, which is provided by Shandong Binzhou Zhiyuan Biotechnology Co., Ltd.

[0044] A preparation method of the concrete composite admixture comprises the following steps: after uniformly mixing the components by weight, adding the components into a ball mill and grinding for 20 minutes, discharging the components to obtain the concrete composite admixture.

[0045] Comparative Example 1

[0046] A concrete composite admixture is substantially the same as Example 1, except that piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), fly ash fiber and 1-benzylpyridine-3-carboxylate are not added.

[0047] Comparative Example 2

[0048] A concrete composite admixture is substantially the same as Example 1, except that no hyperbranched polyglycerol, nano zinc oxide and functional copolymer are added.

[0049] In order to further illustrate the beneficial technical effects of the concrete composite admixtures involved in each embodiment of the present invention, the concrete composite admixtures involved in Examples 1-5 and Comparative Examples 1-2 were tested for relevant performances. The test results are shown in Table 1. The test method is as follows: The concrete composite admixtures prepared in Examples 1-5 and Comparative Examples 1-2 were added to ordinary concrete for performance testing, wherein the amount of the concrete composite admixture was 0.1wt%, and the ordinary concrete ratio was: m (cement): m (fly ash): m (river sand): m (crushed stone): m (water) = 300: 56: 840: 1050: 110. The relevant properties of the obtained concrete were tested with reference to GB / T50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete" and GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". The cement is general PO 52.5 ordinary Portland cement; the fineness modulus of the river sand is 2.5; the crushed stone is a continuously graded stone with a particle size of 5-25 mm. The water reduction rate of each additive is tested and calculated according to the national standard GB8076-2008.

[0050] Table 1

[0051] project Impermeability grade Compressive strength (28d) Water reduction rate Crack area per unit area unit class MPa % <![CDATA[mm 2 / m 2 ]]> Example 1 >P12 72.5 33 88 Example 2 >P12 73.1 35 84 Example 3 >P12 74.3 39 78 Example 4 >P12 75.0 40 73 Example 5 >P12 75.4 42 70 Comparative Example 1 P10 61.8 30 110 Comparative Example 2 P10 59.3 28 103

[0052] As can be seen from Table 1, the concrete composite admixture disclosed in the embodiment of the present invention improves the compressive strength and anti-seepage and anti-cracking performance of concrete more significantly than the comparative example; the addition of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), fly ash fiber, 1-benzylpyridine-3-carboxylate, hyperbranched polyglycerol, nano zinc oxide and functional copolymer is beneficial to improving the above properties.

[0053] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A concrete composite admixture, It is characterized in that The invention comprises the following components in parts by weight: 1-3 parts of tetramethylol glycoluril, 2-4 parts of piperazine-N,N'-bis(2-hydroxypropane sulfonic acid), 1-3 parts of water-soluble polymerized cyclodextrin, 3-5 parts of hyperbranched polyglycerol, 1-3 parts of nano zinc oxide, 1-3 parts of fly ash fiber, 0.8-1.5 parts of 1-benzylpyridine-3-carboxylate, 1-4 parts of surfactant, and 1-2 parts of functional copolymer; the functional copolymer is prepared by free radical copolymerization of 2-acrylamido-2-methylpropane sulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, and 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate; The preparation method of the functional copolymer comprises the following steps: adding 2-acrylamido-2-methylpropanesulfonic acid, 2-vinyl pyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate and an initiator into a high boiling point solvent, stirring and reacting at 50-65° C. in an inert gas atmosphere for 4-6 hours, then removing the solvent by rotary evaporation, washing with ethanol for 3-6 times, and then placing The copolymer is dried in a vacuum drying oven at 85-95° C. to constant weight to obtain a functional copolymer; the mass ratio of the 2-acrylamido-2-methylpropanesulfonic acid, 2-vinylpyrimidine, 2,4-diphenyl-4-methyl-1-pentene, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, initiator, and high boiling point solvent is 3:(1-2):1:(0.8-1.3):(0.06-0.1):(20-30).

2. The concrete composite admixture according to claim 1, It is characterized in that The initiator is azobisisobutyronitrile; the high boiling point solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone; and the inert gas is any one of nitrogen, helium, neon, and argon.

3. The concrete composite admixture according to claim 1, It is characterized in that The surfactant is one or more of fatty alcohol polyoxyethylene ether, nonylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether phosphate.

4. The concrete composite admixture according to claim 1, It is characterized in that The diameter of the fly ash fiber is 1-10 μm; the particle size of the nano zinc oxide is 20-80 nm.

5. A method for preparing the concrete composite admixture according to any one of claims 1 to 4, It is characterized in that The method comprises the following steps: mixing the components uniformly according to weight, adding the components into a ball mill, grinding the components for 10-20 minutes and then discharging the components to obtain a concrete composite admixture.

Citation Information

Patent Citations

  • Method for manufacturing superfine fiber using flyash as raw material

    CN1579978A

  • Concrete complex additive

    CN102153313A

  • Retarding water-reducing crack arresting agent

    CN104119020A

  • Concrete pipe pile and preparation method thereof

    CN105016682A

  • Antibacterial PVC pipe and preparation method thereof

    CN110330737A