Paper-covered copper flat wire and preparation method thereof
Through plasma and sodium nitrite activation treatment and coating with silicon dioxide, silicon carbide and rare earth oxides, combined with hot pressing treatment, the modified aramid insulating paper layer significantly improves the wear resistance and insulation of paper-clad copper flat wires. , solves the problems of easy wear and insufficient insulation performance of single-layer insulating paper, extends the service life and remains stable in high-voltage environments.
Patent Information
- Application Number
- CN202410850896.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The single-layer insulating paper is easy to wear during use, resulting in a short service life of the paper-coated copper flat wire, and insufficient insulation performance, making it difficult to maintain stability in high-voltage and high-electric field environments.
Using plasma surface treatment and sodium nitrite activation of aramid insulating paper, and coating the surface with silicon dioxide, silicon carbide and rare earth oxides, forming a modified aramid insulating paper layer through ultrasonic dispersion and spraying, combined with hot pressing treatment To enhance mechanical strength and insulation properties.
It significantly improves the surface energy, interface bonding force and mechanical strength of the modified aramid insulating paper, extends the service life of the paper-coated copper flat wire, and maintains good insulation performance in high-voltage environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of paper-covered copper flat wires and relates to a paper-covered copper flat wire and a preparation method thereof. Background Art
[0002] Paper-wrapped copper flat wire process is a common wire and cable manufacturing process, mainly used in household appliances, communication equipment, electrical equipment and other fields. This process has the characteristics of simple manufacturing process, good insulation performance, excellent conductivity, etc., so it has been widely used in many fields. In the field of communication equipment, paper-wrapped copper flat wire is usually used in the production of transmission lines such as telephone lines and network cables to ensure stable signal transmission. In addition, it is also widely used in construction, transportation, aerospace and other fields.
[0003] The outer layer of paper-wrapped copper flat wire is usually wrapped with insulating paper. This insulating paper has good insulation performance and high temperature resistance, which can ensure that the copper flat wire maintains stable electrical performance during use and prevent problems such as current leakage or short circuit. At the same time, the insulating paper can also provide additional mechanical protection to enhance the durability and reliability of the copper flat wire. However, a single layer of insulating paper is prone to wear during use, resulting in a short service life of the paper-wrapped copper flat wire. In order to solve the above problems, the insulating paper is modified to improve its wear resistance and insulation. Summary of the invention
[0004] The object of the present invention is to provide a paper-covered copper rectangular wire and a preparation method thereof, which has the characteristics of good wear resistance and high insulation.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A paper-covered copper rectangular wire comprises an inner metal copper conductor and an outer modified aramid insulation paper layer. The preparation process of the modified aramid insulation paper layer is as follows:
[0007] S1: The aramid insulation paper was placed at room temperature and pressure in a nitrogen atmosphere and subjected to plasma surface treatment for 120 seconds using a 400W power supply;
[0008] S2: Sodium nitrite with a mass concentration of 10% is evenly coated on the aramid insulation paper treated with plasma, and then washed with deionized water after leaving it for 20 minutes, and then purged with active oxygen gas at 60°C at a flow rate of 10m / s for 2 hours to dry the surface of the aramid insulation paper;
[0009] S3: mixing silicon dioxide, silicon carbide and rare earth oxide in a mass ratio of 1:1:1, and grinding the mixture in a ball mill at a speed of 300 r / min for 2 h to obtain a mixture;
[0010] S4: dispersing the mixture in deionized water to obtain a solid-liquid mixture A with a mass concentration of 30%, and ultrasonicating the solid-liquid mixture A for 1 h to obtain a uniformly dispersed solid-liquid mixture B;
[0011] S5: spraying the solid-liquid mixture B prepared in S4 uniformly on the surface of the aramid insulation paper prepared in S2, and drying it by laser irradiation;
[0012] S6: hot-pressing the aramid insulation paper obtained in S5 at 70° C., with a pressure of 500-700 N and a hot-pressing time of 200-300 s, and standing for 12 hours after hot-pressing to obtain the modified aramid insulation paper layer.
[0013] Furthermore, the spraying parameters of the solid-liquid mixture B in S5 are a spraying distance of 80 mm and a spraying rate of 60 mm / s.
[0014] Furthermore, the rare earth oxide in S3 is one or more of cerium oxide, lanthanum oxide, and praseodymium oxide.
[0015] Furthermore, the powder obtained by grinding in S3 has a particle size of 300-400 meshes.
[0016] Furthermore, the laser irradiation parameters in S5 are: laser power 250W, temperature 80°C, and irradiation time 30min.
[0017] Furthermore, the thickness of the modified aramid insulation paper layer prepared by S6 is 0.8~1.2mm.
[0018] A method for preparing a paper-covered copper flat wire, the preparation process of the paper-covered copper flat wire is as follows:
[0019] S71: Drawing the metal copper wire through a flat die on a wire drawing device, and then rolling it through a rolling die on the wire drawing device to obtain a copper flat wire;
[0020] S72: transferring the copper flat wire after drawing and rolling into an annealing furnace, and annealing at a speed of 150 m / min in a nitrogen atmosphere;
[0021] S73: using an ultrasonic cleaning machine to ultrasonically clean the annealed copper flat wire to obtain a clean copper flat wire;
[0022] S74: using nitrogen gas at 50° C. at a flow rate of 8 m / s to purge the copper flat wire to obtain a copper flat wire with a dry and clean surface;
[0023] S75: Wrapping the modified aramid insulation paper layer on the outside of the copper flat wire to obtain the final product, paper-wrapped copper flat wire.
[0024] Furthermore, the thickness of the copper flat wire obtained in S71 is 2.7 mm.
[0025] The present invention first treats the surface of the aramid insulating paper by plasma. The active ions in the plasma can bombard the aramid surface, causing its surface structure to undergo subtle adjustments, thereby improving the interfacial bonding strength of the insulating paper. This optimized surface performance helps to enhance the compatibility of the insulating paper with other materials, and improves the stability and reliability of the overall system. Plasma treatment can also effectively reduce the dielectric constant and dielectric loss of the insulating paper, improve its electrical strength, and enable the insulating paper to maintain good insulation performance in harsh environments such as high voltage and high electric field strength.
[0026] Sodium nitrite and active oxygen gas are then used to activate the surface of the aramid insulation paper. The activation treatment can enhance the bonding force between fibers, improve the tensile strength and tear strength of the insulation paper, while maintaining its good thermal stability. The sodium nitrite treatment can significantly increase the surface energy of the aramid insulation paper, and the increase in surface energy helps to enhance the adhesion between the insulation paper and other materials. Sodium nitrite reacts chemically with the surface of the aramid fiber to introduce new functional groups, which can increase the reactivity of the insulation paper surface. The active oxygen gas is then used to further activate the surface energy of the aramid insulation paper, so that the interfacial bonding force between the aramid insulation paper and the metal conduit is significantly improved, and the prepared paper-wrapped copper flat wire has higher stability. The activation treatment can also improve the wettability and coating properties of the aramid insulation paper, which makes it easier to achieve uniform coverage and close fit when the insulation paper is coated on other materials.
[0027] The present invention coats a layer of mixed solution of silicon dioxide, silicon carbide and rare earth oxide on the surface of the activated aramid insulation paper, thereby further improving the mechanical strength of the aramid insulation paper. Silicon carbide, as a high-hardness material, can effectively enhance the structure of the aramid insulation paper, making its surface harder and less prone to wear; and the addition of rare earth oxide can effectively improve the insulation performance of the aramid insulation paper and promote material compounding, so that the combination of silicon dioxide, silicon carbide and aramid insulation paper is tighter; rare earth oxide also has certain anti-oxidation and anti-aging properties, which can delay the aging process of the aramid insulation paper during use and extend the service life of the prepared paper-covered copper flat wire.
[0028] The present invention strengthens the acting force between aramid cellulose chains by means of hot pressing, makes the combination tighter, and increases the linear density, thereby significantly improving the tear index and tensile index of the aramid insulation paper.
[0029] Beneficial effects of the present invention:
[0030] The present invention uses a plasma method to modify the surface and activates the surface of the aramid insulation paper in combination with sodium nitrite and active oxygen gas, thereby significantly improving the surface energy of the aramid insulation paper, significantly improving the interface bonding force between the aramid insulation paper and the metal conduit, and making the prepared paper-wrapped copper flat wire have higher stability; the present invention further improves the mechanical strength and oxidation resistance of the aramid insulation paper by coating a layer of a mixed solution of silicon dioxide, silicon carbide and rare earth oxide on the surface of the aramid insulation paper, and prolongs the service life of the prepared paper-wrapped copper flat wire; the present invention strengthens the force between the aramid cellulose chains by hot pressing, makes the bonding more tight, and increases the line density, thereby significantly improving the tear index and tensile index of the aramid insulation paper. DETAILED DESCRIPTION
[0031] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0032] Example 1
[0033] The preparation process of the modified aramid insulation paper layer is as follows:
[0034] S1: The aramid insulation paper was placed at room temperature and pressure in a nitrogen atmosphere and subjected to plasma surface treatment for 120 seconds using a 400W power supply;
[0035] S2: Sodium nitrite with a mass concentration of 10% is evenly coated on the aramid insulation paper treated with plasma, and then washed with deionized water after leaving it for 10 minutes, and then purged with active oxygen gas at 60°C at a flow rate of 10m / s for 2 hours to dry the surface of the aramid insulation paper;
[0036] S3: mixing silicon dioxide, silicon carbide and lanthanum oxide in a mass ratio of 1:1:1, and grinding them in a ball mill at a speed of 300 r / min for 2 h to obtain a mixture;
[0037] S4: dispersing the mixture in deionized water to obtain a solid-liquid mixture A with a mass concentration of 30%, and ultrasonicating the solid-liquid mixture A for 1 h to obtain a uniformly dispersed solid-liquid mixture B;
[0038] S5: The solid-liquid mixture B prepared in S4 is uniformly sprayed on the surface of the aramid insulation paper prepared in S2 at a spraying distance of 80 mm and a spraying rate of 60 mm / s, and then dried by laser irradiation. The laser power is 250 W, the temperature is 80 ° C, and the irradiation time is 30 min.
[0039] S6: hot-pressing the aramid insulation paper obtained in S5 at 70° C., with a pressure of 500 N and a hot-pressing time of 300 s, and standing for 12 hours after hot-pressing to obtain the modified aramid insulation paper layer.
[0040] The preparation process of the paper-covered copper flat wire is as follows:
[0041] S71: Drawing the metal copper wire through a flat die on a wire drawing device, and then rolling it through a rolling die on the wire drawing device to obtain a copper flat wire;
[0042] S72: transferring the copper flat wire after drawing and rolling into an annealing furnace, and annealing at a speed of 150 m / min in a nitrogen atmosphere;
[0043] S73: using an ultrasonic cleaning machine to ultrasonically clean the annealed copper flat wire to obtain a clean copper flat wire;
[0044] S74: using nitrogen gas at 50° C. at a flow rate of 8 m / s to purge the copper flat wire to obtain a copper flat wire with a dry and clean surface;
[0045] S75: Wrapping the modified aramid insulation paper layer on the outside of the copper flat wire to obtain the final product, paper-wrapped copper flat wire.
[0046] In Example 2, the pressure in S6 is 700N, the hot pressing time is 200s, and the other conditions are the same as in Example 1.
[0047] In Comparative Example 1, the aramid insulation paper is not subjected to S1 plasma surface treatment, and other conditions are the same as those in Example 1.
[0048] In Comparative Example 2, the aramid insulation paper is not subjected to S2 surface activation treatment, and other conditions are the same as those in Example 1.
[0049] In Comparative Example 3, the aramid insulation paper is not subjected to the S5 surface mixed liquid coating treatment, and other conditions are the same as those in Example 1.
[0050] In Comparative Example 4, the aramid insulation paper is not subjected to S6 hot pressing treatment, and other conditions are the same as those in Example 1.
[0051] The mechanical strength test of the prepared paper-covered copper flat wire was carried out according to GB / T 4074.3-2008. The specific test method is as follows:
[0052] Install the test sample on the tensile testing machine, making sure that the installation direction of the sample is consistent with the tensile direction;
[0053] Set the stretching speed to 2 mm / s, the stretching force to 200 N, and the stretching time to 20 s;
[0054] The stretching was recorded and the sample tensile strength was analyzed.
[0055] The bending modulus test of the prepared paper covered copper flat wire was carried out according to GB / T 9341-2008. The paper covered copper flat wire sample was fixed on the fixture of the bending tester to ensure that the sample would not slide or shift during the test. A constant bending force was applied to the sample through the testing equipment to cause bending deformation.
[0056] The conductivity of the test sample is tested according to GB / T 17650.2-2021 standard. The lower the conductivity, the better the insulation.
[0057] The experimental results of the embodiments and comparative examples are summarized in the following table:
[0058]
[0059] It can be seen from the experimental results that the modification of aramid insulation paper effectively improves the mechanical strength and insulation of the obtained paper-covered copper rectangular wire, among which Example 1 is the best example.
[0060] When the present invention is used:
[0061] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A paper-covered copper rectangular wire, comprising an inner metal copper conductor and an outer modified aramid insulating paper layer, characterized in that: The preparation process of the modified aramid insulation paper layer is as follows: S1: The aramid insulation paper was placed at room temperature and pressure in a nitrogen atmosphere and subjected to plasma surface treatment for 120 seconds using a 400W power supply; S2: Sodium nitrite with a mass concentration of 10% is evenly coated on the aramid insulation paper treated with plasma, and then washed with deionized water after leaving it for 10 minutes, and then purged with active oxygen gas at 60°C at a flow rate of 10m / s for 2 hours to dry the surface of the aramid insulation paper; S3: mixing silicon dioxide, silicon carbide and rare earth oxide in a mass ratio of 1:1:1, and grinding them in a ball mill at a speed of 300 r / min for 2 h to obtain a mixture; S4: dispersing the mixture in deionized water to obtain a solid-liquid mixture A with a mass concentration of 30%, and ultrasonicating the solid-liquid mixture A for 1 h to obtain a uniformly dispersed solid-liquid mixture B; S5: spraying the solid-liquid mixture B prepared in S4 uniformly on the surface of the aramid insulation paper prepared in S2, and drying it by laser irradiation; S6: hot-pressing the aramid insulation paper obtained in S5 at 70° C., with a pressure of 500-700 N and a hot-pressing time of 200-300 s, and standing for 12 hours after hot-pressing to obtain the modified aramid insulation paper layer.
2. The paper-covered rectangular copper wire according to claim 1, characterized in that: The spraying parameters of the solid-liquid mixture B in S5 are a spraying distance of 80 mm and a spraying rate of 60 mm / s.
3. The paper covered rectangular copper wire according to claim 1, characterized in that: The rare earth oxide in S3 is one or more of cerium oxide, lanthanum oxide and praseodymium oxide.
4. The paper covered rectangular copper wire according to claim 1, characterized in that: The powder obtained by grinding in S3 has a particle size of 300-400 meshes.
5. The paper covered rectangular copper wire according to claim 1, characterized in that: The laser irradiation parameters in S5 are: laser power 250 W, temperature 80° C., and irradiation time 30 min.
6. The paper covered rectangular copper wire according to claim 1, characterized in that: The thickness of the modified aramid insulation paper layer prepared by S6 is 0.8-1.2 mm.
7. A method for preparing a paper-covered copper flat wire, based on the paper-covered copper flat wire according to any one of claims 1 to 6, characterized in that: The preparation process of the paper-covered copper flat wire is as follows: S71: Drawing the metal copper wire through a flat die on a wire drawing device, and then rolling it through a rolling die on the wire drawing device to obtain a copper flat wire; S72: transferring the copper flat wire after drawing and rolling into an annealing furnace, and annealing at a speed of 150 m / min in a nitrogen atmosphere; S73: using an ultrasonic cleaning machine to ultrasonically clean the annealed copper flat wire to obtain a clean copper flat wire; S74: using nitrogen gas at 50° C. at a flow rate of 8 m / s to purge the copper flat wire to obtain a copper flat wire with a dry and clean surface; S75: Wrapping the modified aramid insulation paper layer on the outside of the copper flat wire to obtain the final product, paper-wrapped copper flat wire.
8. The method for preparing a paper-covered rectangular copper wire according to claim 7, characterized in that: The thickness of the copper flat wire obtained in S71 is 2.7 mm.
Citation Information
Patent Citations
Preparation method of aramid fiber nano-mica insulation paper modified by plasma treatment
CN111945478A
Method for treating aramid fiber doped modified cellulose insulation paper by plasma
CN113789681A
Inorganic nano-material reinforced aramid insulation paper and preparation method and application thereof
CN115045140A
Heat-aging-resistant aramid insulation paper and preparation method thereof
CN115058916A
Preparation method of copolymerized self-coloring aramid fiber and copolymerized self-coloring aramid fiber