Back contact cell with enhanced reflection structure, manufacturing method thereof and photovoltaic module

By arranging an anti-reflection layer in the back contact battery, the problem of the metal layer absorbing light in the near-infrared band is solved, the short-circuit current and conversion efficiency of the battery are improved, and more efficient use of light energy is achieved.

CN118398696BActive Publication Date: 2024-10-29GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410851548.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

When the existing back-contact battery is plated with a metal layer on the transparent conductive film layer, the near-infrared band light is absorbed by the metal layer, resulting in a problem of reduced short-circuit current.

Method used

An anti-reflection layer is placed between the transparent conductive film layer and the metal layer to form a specific anti-reflection structure, which reduces the metal layer's absorption of near-infrared free carriers, increases the absorption rate and reflectivity of light, and increases the short-circuit current of the battery. and conversion efficiency.

Benefits of technology

Through the design of the anti-reflective layer, the absorption rate and reflectivity of light are increased, and the short-circuit current and conversion efficiency of the battery are improved, especially in the near-infrared band, which significantly improves the performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398696B_ABST
    Figure CN118398696B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of back contact batteries, and specifically relates to a back contact battery with a reflection enhancement structure, a manufacturing method thereof, and a photovoltaic module, comprising a battery substrate with a semiconductor distribution layer on the back, and a transparent conductive film layer and a metal layer sequentially arranged on the outer surface of the semiconductor distribution layer, wherein the semiconductor distribution layer comprises an N-type conductive region and a P-type conductive region arranged alternately, and further comprises a reflection enhancement layer arranged between the transparent conductive film layer and the metal layer, wherein the reflection enhancement layer and the transparent conductive film layer form a reflection enhancement structure, and the reflection enhancement structure satisfies: n2 is less than n1, n2 is 1.4-1.8, and complies with the following corresponding relationship d1×n1+d2×n2=D. The present invention can increase the light absorption rate, reduce the free carrier absorption (FCA) of the metal layer to the near infrared, and increase the reflection of the near infrared band, so as to improve the absorption of the battery substrate to the near infrared band, and improve the short-circuit current and battery conversion efficiency of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back contact cells, and in particular relates to a back contact cell provided with a reflection enhancement structure, a manufacturing method thereof, and a photovoltaic module. Background Art

[0002] At present, back-contact heterojunction solar cells or back-contact cells with combined passivation generally use silver paste fine grids as the back electrodes. In order to save the cost of silver paste, a back-plated metal layer (generally copper plating or composite metal layer) is used to replace the silver paste fine grid, or to replace part of the silver paste fine grid to enhance the conductivity. The manufacturing method is generally as follows: a transparent conductive film layer is deposited on the surface of the back semiconductor distribution layer, and then a metal layer (such as PVD sputtering Cu) is deposited on the transparent conductive film layer.

[0003] However, if a metal layer is directly plated on the transparent conductive film layer, the light in the near-infrared band will pass through the silicon substrate of the battery and will be directly absorbed into the metal layer. Since the metal contains a large number of free carriers, the free carriers will produce free-carrier absorption (FCA for short). This part of the light is absorbed by the metal layer and lost, which greatly affects the near-infrared reflection of the back of the battery. This phenomenon will lead to the following disadvantages: the full area coverage of the metal copper layer will reduce the near-infrared reflection that the silicon of the battery body can absorb, thereby reducing the short-circuit current.

[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defect of low short-circuit current of the back-contact battery in the prior art in which a metal layer is deposited on a transparent conductive film layer to form an electrode, and to provide a back-contact battery with a reflection-enhancing structure, a method for manufacturing the same, and a photovoltaic module. The back-contact battery can increase the light absorption rate, reduce the free carrier absorption (FCA) of the metal layer to the near-infrared, increase the reflection of the near-infrared band, so as to improve the absorption of the battery substrate to the near-infrared band, and improve the short-circuit current of the battery and the battery conversion efficiency.

[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a back contact battery with a reflection enhancement structure, comprising a battery substrate with a semiconductor distribution layer on the back, and a transparent conductive film layer and a metal layer sequentially arranged on the outer surface of the semiconductor distribution layer, wherein the semiconductor distribution layer comprises an N-type conductive region and a P-type conductive region arranged alternately, and further comprises a reflection enhancement layer arranged between the transparent conductive film layer and the metal layer, wherein the reflection enhancement layer and the transparent conductive film layer form a reflection enhancement structure, and the reflection enhancement structure satisfies:

[0007] n2 is smaller than n1, n2 is 1.4-1.8, and meets the following corresponding relationship d1×n1+d2×n2=D, and the value range of D is 200-300nm;

[0008] Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm.

[0009] In some preferred embodiments of the present invention, d1 is 40-150 nm, and n1 is 1.55-2.2.

[0010] In some preferred embodiments of the present invention, d2 is 10-150 nm.

[0011] In some preferred embodiments of the present invention, the ratio of n2 to n1 is 0.65-0.9:1.

[0012] In some preferred embodiments of the present invention, the material of the reflection-enhancing layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, titanium oxide, tin oxide, and zinc oxide.

[0013] In some preferred embodiments of the present invention, the material of the reflection-enhancing layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide.

[0014] In some preferred embodiments of the present invention, openings are provided on the reflection-enhancing layer, the openings are distributed in separate points or in continuous lines, and the openings are filled with a metal material corresponding to the metal layer.

[0015] In some preferred embodiments of the present invention, the openings of the reflection-enhancing layer are distributed in a continuous linear shape, and the openings are extended along the length direction of the corresponding N-type conductive region or P-type conductive region.

[0016] Preferably, the opening area of ​​the reflection-enhancing layer is 10%-30% of the area of ​​the corresponding N-type conductive region or P-type conductive region.

[0017] Preferably, the openings of the reflection-enhancing layer consist of a plurality of openings parallel to the N-type conductive region or the P-type conductive region, and the total width of the plurality of openings is 10%-30% of the width of the corresponding N-type conductive region or the P-type conductive region.

[0018] In some preferred embodiments of the present invention, the ratio of the total thickness of the reflection-enhancing structure to the thickness of the corresponding metal layer on the outer surface of the reflection-enhancing layer is 0.3-0.8:1, and / or the thickness of the corresponding metal layer on the outer surface of the reflection-enhancing layer is 150-450 nm.

[0019] In some preferred embodiments of the present invention, the back contact cell with a reflection enhancement structure further has at least one of the following structures:

[0020] Structure 1: The back contact cell with a reflection enhancement structure further includes an anti-oxidation protective layer disposed on the outer surface of the metal layer;

[0021] Structure 2: The material of the metal layer includes at least one of copper, silver, tin and gold;

[0022] Structure 3: The N-type conductive region includes a first passivation layer and an N-type semiconductor layer, the P-type conductive region includes a second passivation layer and a P-type semiconductor layer, and the first passivation layer and the second passivation layer are independently selected from an intrinsic silicon layer or a tunneling oxide layer.

[0023] In a second aspect, the present invention provides a method for manufacturing a back contact battery, comprising the following steps:

[0024] S1. Providing a battery substrate with a semiconductor distribution layer on the back side, wherein the semiconductor distribution layer comprises N-type conductive regions and P-type conductive regions arranged alternately;

[0025] S2, depositing a transparent conductive film layer on the outer surface of the semiconductor distribution layer;

[0026] S3. Depositing a reflection-enhancing layer on the outer surface of the transparent conductive film layer. The reflection-enhancing layer and the transparent conductive film layer form a reflection-enhancing structure. The reflection-enhancing structure is controlled to meet the following requirements:

[0027] n2 is smaller than n1 and meets the following corresponding relationship: d1×n1+d2×n2=D, and the value range of D is 200-300nm;

[0028] Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm;

[0029] S4. Depositing a metal layer on the outer surface of the reflection enhancing layer.

[0030] In some preferred embodiments of the present invention, the material of the reflective enhancement layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, and the method for manufacturing the back contact battery also includes: after depositing the reflective enhancement layer in S3, the reflective enhancement layer is partially opened, and the openings are distributed in separate points or in continuous lines, and then S4 metal layer is deposited.

[0031] In some preferred embodiments of the present invention, the method for manufacturing the back contact battery further includes: S5, depositing an anti-oxidation protective layer on the outer surface of the metal layer.

[0032] In a third aspect, the present invention provides a back-contact battery, which is manufactured by the method for manufacturing a back-contact battery described in the second aspect.

[0033] In a fourth aspect, the present invention provides a photovoltaic module, which includes the back contact cell provided with a reflection enhancement structure as described in the first aspect, or includes the back contact cell as described in the third aspect.

[0034] Beneficial effects:

[0035] The present invention adopts the above technical scheme, especially adds a reflection-enhancing layer between the transparent conductive film layer and the metal layer to form a specific reflection-enhancing structure, so that part of the light will be reflected back to the battery substrate at the interface between the transparent conductive film layer and the reflection-enhancing layer, thereby increasing the probability of light being absorbed to excite electron-hole pairs, thereby increasing the light absorption rate and improving the short-circuit current (abbreviated as Isc); the reflection-enhancing layer cooperates with the metal layer to reduce the free carrier absorption (FCA) of the metal layer to the near-infrared, increase the reflection of the near-infrared band, so as to improve the absorption of the battery substrate to the near-infrared band, and further improve the short-circuit current and battery conversion efficiency of the battery. Among them, the present invention also cooperates with controlling n2 to be less than n1, n2 is 1.4-1.8, which can make the light go from a denser medium to a less dense medium, and meet the following corresponding relationship d1×n1+d2×n2=D, and the value range of D is 200-300nm, so that the total thickness of the reflection-enhancing structure is 1 / 4 of the target wavelength, thereby having the best reflection-enhancing effect near a wavelength of 1000nm, and can achieve minimum transmission and maximum reflection of specific wavelength light in the near-infrared band of 800-1200nm.

[0036] In the preferred embodiment of the present invention, the material of the reflective layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, and openings are also provided on the reflective layer to enhance the collection and transmission of current and further increase the short-circuit current. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 A schematic structural diagram of a specific implementation of a back contact battery.

[0039] Figure 2 It is a schematic structural diagram of another specific implementation of a back contact battery.

[0040] Figure 3This is a comparison curve of substrate absorption rates corresponding to different back structures of back-contact batteries.

[0041] Description of Reference Numerals

[0042] 1. Battery substrate, 2. Transparent conductive film layer, 3. Reflection enhancement layer, 4. Metal layer, 5. Anti-oxidation protection layer. DETAILED DESCRIPTION

[0043] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0044] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0045] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0046] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0047] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.

[0048] In a first aspect, the present invention provides a back-contact battery with a reflection-enhancing structure, comprising a battery substrate with a semiconductor distribution layer on the back, and a transparent conductive film layer and a metal layer sequentially arranged on the outer surface of the semiconductor distribution layer, wherein the semiconductor distribution layer comprises an N-type conductive region and a P-type conductive region arranged alternately, and further comprises a reflection-enhancing layer arranged between the transparent conductive film layer and the metal layer, wherein the reflection-enhancing layer and the transparent conductive film layer form a reflection-enhancing structure, and the reflection-enhancing structure satisfies:

[0049] n2 is smaller than n1, n2 is 1.4-1.8, preferably 1.4-1.6, and meets the following corresponding relationship d1×n1+d2×n2=D, and the value range of D is 200-300nm, preferably 200-270nm;

[0050] Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm.

[0051] In the present invention, the average refractive index is measured by using a spectroscopic ellipsometer.

[0052] In some preferred embodiments of the present invention, d1 is 40-150nm, and n1 is 1.55-2.2. A transparent conductive film layer with a suitable thickness and average refractive index is used. First, a transparent conductive film layer with a sufficient thickness is ensured to collect current. At the same time, the refractive index of the reflective enhancement layer is slightly higher than that of the reflective enhancement layer, so that the light can be set gradually from the optically dense medium to the optically sparse medium. Combined with the film thickness relationship setting, the maximum reflective enhancement effect of the light in the target wavelength region can be achieved.

[0053] In the present invention, preferably, d2 is 10-150 nm.

[0054] In some preferred embodiments of the present invention, the ratio of n2 to n1 is 0.65-0.9: 1, preferably 0.65-0.85: 1. The use of a reflective enhancement layer and a transparent conductive film layer with a suitable refractive index ratio is more conducive to the appropriate transmission of light from a denser medium to a less dense medium, and combined with the corresponding film thickness relationship setting, the maximum reflective enhancement effect on light in the target wavelength region is achieved.

[0055] In some preferred embodiments of the present invention, the material of the reflection-enhancing layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, titanium oxide, tin oxide, and zinc oxide.

[0056] In some embodiments, taking the three schemes of the reflective layer being made of silicon oxide and having an opening in the reflective layer (the area of ​​the opening is 10% of the area of ​​the corresponding N-type conductive region or P-type conductive region), the reflective layer being made of tin oxide, and no reflective layer being provided as examples (in different schemes, the structures other than the reflective layer are the same), the Waferray tracer tool provided by PVlighthouse is used to simulate the absorption of light of different wavelengths of the back contact cells of the three schemes, which can more intuitively reflect the effect of the reflective layer. The results are as follows: Figure 3 As shown, the larger the area enclosed by the curve, the more light is absorbed. Figure 3 It can be seen that the enclosed area of ​​the solution in which the material of the reflective enhancement layer is silicon oxide>the solution in which the material of the reflective enhancement layer is tin oxide>no reflective enhancement layer is provided. The main difference among the three is in the absorption rate of light with a wavelength between 800nm ​​and 1200nm, which shows that adding the reflective enhancement layer has a significant effect on the absorption of light in theory.

[0057] In some preferred embodiments of the present invention, the material of the reflection-enhancing layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide.

[0058] In an embodiment of the present invention where the material of the reflective enhancement layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, preferably, an opening is provided on the reflective enhancement layer, and the opening is filled with a metal material corresponding to the metal layer, which is more conducive to enhancing the collection and transmission of current.

[0059] In some preferred embodiments of the present invention, the opening area of ​​the reflective enhancement layer is 10%-30%, preferably 10%-20%, of the area of ​​the corresponding N-type conductive region or P-type conductive region. With this preferred solution, the opening area is appropriate, so that the contact area between the transparent conductive film layer and the metal layer is appropriately large, the contact resistance is reduced, the series resistance is increased, and at the same time, a relatively high area of ​​the reflective enhancement effect is maintained, further increasing the short-circuit current.

[0060] The opening area of ​​the reflective enhancement layer is 10%-30% of the area of ​​the corresponding N-type conductive region or P-type conductive region, which means that the total area of ​​the opening of the reflective enhancement layer accounts for 10%-30% of the area of ​​the N-type conductive region or P-type conductive region corresponding to the opening. Exemplarily, the opening area on the N-type conductive region is 10%-30% of the area of ​​the N-type conductive region, and the opening area on the P-type conductive region is 10%-30% of the area of ​​the P-type conductive region.

[0061] Furthermore, the openings are distributed in separate point shapes or in continuous line shapes.

[0062] Preferably, the openings are distributed in a continuous linear manner, and the openings are extended along the length direction of the N-type conductive region or the P-type conductive region. Further preferably, the width of the openings is 10%-30%, preferably 10%-20%, of the width of the corresponding N-type conductive region or the P-type conductive region.

[0063] In some specific embodiments, the openings are distributed in separate dot-like shapes, and the openings are evenly distributed along the length direction and / or width direction of the N-type conductive region or the P-type conductive region. Further preferably, the openings of the reflective enhancement layer are composed of a plurality of openings parallel to the N-type conductive region or the P-type conductive region, and the total width of the plurality of openings is 10%-30%, preferably 10%-20%, of the width of the corresponding N-type conductive region or the P-type conductive region.

[0064] The total width of the multiple openings is 10%-30% of the width of the corresponding N-type conductive region or P-type conductive region, which means that in the same width direction, the sum of the widths of all openings of the reflective enhancement layer is 10%-30% of the width of the corresponding N-type conductive region or P-type conductive region in the area where they are located.

[0065] In the solution of the present invention where the material of the reflective enhancement layer is tin oxide and / or zinc oxide, since the two materials themselves have good electrical conductivity, when the reflective enhancement layer is relatively thin, no openings need to be provided to ensure better conductivity, which is beneficial to the simplified application of the battery manufacturing process and achieves the reflective enhancement effect on the back of the battery.

[0066] Preferably, the ratio of the total thickness of the reflection-enhancing structure to the thickness of the corresponding metal layer located on the outer surface of the reflection-enhancing layer is 0.3-0.8: 1. This preferred solution is more conducive to controlling the appropriate total thickness of the reflection-enhancing structure to avoid the stress and other factors of the overly thick bottom multi-layer structure affecting the adhesion of the metal layer and causing defects such as film layer shedding.

[0067] Preferably, the thickness of the corresponding metal layer on the outer surface of the reflection-enhancing layer is 150-450 nm. It is understandable that the thickness of the corresponding metal layer on the outer surface of the reflection-enhancing layer and the local metal layer corresponding to the opening may be different, and the thickness of the local metal layer corresponding to the opening may be thicker.

[0068] In some preferred embodiments of the present invention, the back contact cell with a reflection enhancement structure further comprises an anti-oxidation protection layer disposed on the outer surface of the metal layer.

[0069] The thickness and material of the anti-oxidation protective layer can refer to the prior art, and can be used in the present invention. In some preferred embodiments of the present invention, the thickness of the anti-oxidation protective layer is 20-50 nm. The material of the anti-oxidation protective layer can be, for example, ITO.

[0070] In some preferred embodiments of the present invention, the material of the metal layer includes at least one of copper, silver, tin and gold.

[0071] The N-type conductive region and the P-type conductive region of the present invention may be doped semiconductor layers formed by doping on a silicon wafer, or may be corresponding semiconductor film layers additionally deposited on the back side of the silicon wafer.

[0072] In some preferred embodiments of the present invention, the N-type conductive region includes a first passivation layer and an N-type semiconductor layer, the P-type conductive region includes a second passivation layer and a P-type semiconductor layer, and the first passivation layer and the second passivation layer are each independently selected from an intrinsic silicon layer or a tunneling oxide layer. For example, a conventional heterojunction structure in which the first passivation layer and the second passivation layer are both intrinsic silicon layers, or a combined passivation structure in which the first passivation layer is a tunneling oxide layer and the second passivation layer is an intrinsic silicon layer, etc., can be used in the present invention.

[0073] In the present invention, the specific distribution structure of the N-type conductive region and the P-type conductive region can refer to any structure of the prior art and can be used in the present invention. For example, it can be two semiconductor conductive regions that are alternately arranged and do not overlap in the thickness direction, or it can be two semiconductor conductive regions that are alternately arranged and partially overlap in the thickness direction. The specific structure of the latter can be: the two ends of the P-type conductive region respectively extend outward to cover the back side of the adjacent N-type conductive region, and a first semiconductor opening region that does not cover the P-type conductive region is opened on the back side of the N-type conductive region, and a second semiconductor opening region is formed between the adjacent N-type conductive regions. The second semiconductor opening region is arranged at an interval with the first semiconductor opening region and the area between them is a spacing region; in the spacing region, a mask layer is set between the N-type conductive region and the P-type conductive region, or no mask layer is set.

[0074] In a second aspect, the present invention provides a method for manufacturing a back contact battery, comprising the following steps:

[0075] S1. Providing a battery substrate with a semiconductor distribution layer on the back side, wherein the semiconductor distribution layer comprises N-type conductive regions and P-type conductive regions arranged alternately;

[0076] S2, depositing a transparent conductive film layer on the outer surface of the semiconductor distribution layer;

[0077] S3. Depositing a reflection-enhancing layer on the outer surface of the transparent conductive film layer. The reflection-enhancing layer and the transparent conductive film layer form a reflection-enhancing structure. The reflection-enhancing structure is controlled to meet the following requirements:

[0078] n2 is smaller than n1 and meets the following corresponding relationship: d1×n1+d2×n2=D, and the value range of D is 200-300nm;

[0079] Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm;

[0080] S4. Depositing a metal layer on the outer surface of the reflection enhancing layer.

[0081] In some preferred embodiments of the present invention, the material of the reflective enhancement layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, and the method for manufacturing the back contact battery also includes: after depositing the reflective enhancement layer in S3, the reflective enhancement layer is partially opened, and the openings are distributed in separate points or in continuous lines, and then S4 metal layer is deposited.

[0082] The deposition method of the reflective enhancement layer of the present invention can be any method in the prior art, as long as a reflective enhancement layer of the desired thickness and refractive index is obtained, for example, it can be any method of physical vapor deposition (including sputtering coating, evaporation coating), chemical vapor deposition, and reactive plasma coating.

[0083] In the present invention, the method for partially opening the reflection-enhancing layer may be, for example, a method of setting a mask layer in combination with an etching solution to perform etching opening, or other existing methods capable of removing the reflection-enhancing layer.

[0084] In the present invention, the corresponding refractive indexes of the transparent conductive film layer and the reflective enhancement layer can be adjusted by the methods in the prior art. As long as the average refractive index within the target wavelength range is within the scope of the present invention, the effect of the present invention can be achieved. For example, the refractive index of the reflective enhancement layer is related to the material type and the deposition conditions (such as deposition method, deposition atmosphere ratio, pressure, speed, etc.). In the present invention, as long as the refractive index can be controlled within the scope of the present invention, it will not be repeated here.

[0085] In some preferred embodiments of the present invention, the method for manufacturing the back contact battery further includes: S5, depositing an anti-oxidation protective layer on the outer surface of the metal layer. The method for depositing the anti-oxidation protective layer can refer to the prior art and will not be described in detail here.

[0086] In a third aspect, the present invention provides a back-contact battery, which is manufactured by the method for manufacturing a back-contact battery described in the second aspect.

[0087] In a fourth aspect, the present invention provides a photovoltaic module, which includes the back contact cell provided with a reflection enhancement structure as described in the first aspect, or includes the back contact cell as described in the third aspect.

[0088] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0089] Example 1

[0090] A back contact battery, such as Figure 2 As shown, the production method is as follows:

[0091] S1. Provide a battery substrate 1 with a semiconductor distribution layer on the back side, wherein the semiconductor distribution layer comprises N-type conductive regions and P-type conductive regions arranged alternately; the N-type conductive regions and the P-type conductive regions are heterojunction passivation structures, and both the N-type conductive regions and the P-type conductive regions are passivation structures of intrinsic amorphous silicon and corresponding doped amorphous silicon layers.

[0092] S2, depositing a transparent conductive film layer 2 on the outer surface of the semiconductor distribution layer; the transparent conductive film layer 2 is a transparent conductive film ITO. The thickness d1 of the transparent conductive film layer 2 is 100 nm, and the average refractive index n1 of the transparent conductive film layer 2 between the wavelength of 800 nm and 1200 nm is 2.0.

[0093] S3, depositing a reflection-enhancing layer 3 on the outer surface of the transparent conductive film layer 2, and then partially opening the reflection-enhancing layer 3; the local opening is performed by setting a mask layer in combination with an etching solution to perform etching opening.

[0094] The material of the reflective enhancement layer 3 is silicon dioxide, and the openings are distributed in a continuous linear shape. The openings extend along the length direction of the corresponding N-type conductive region or P-type conductive region, and the opening area of ​​the reflective enhancement layer 3 is 10% of the area of ​​the corresponding N-type conductive region or P-type conductive region. Accordingly, the widths of the N-type conductive region and the P-type conductive region are both 500μm, and the width of the opening is 50μm.

[0095] The thickness d2 of the reflection-enhancing layer 3 is controlled to be 40 nm, and the average refractive index n2 of the reflection-enhancing layer 3 between the wavelength of 800 nm and 1200 nm is 1.45. After calculation, d1×n1+d2×n2=D=258 nm. The ratio of n2 to n1 is 0.725:1.

[0096] S4, depositing a metal layer 4 on the outer surface of the reflection-enhancing layer 3, wherein the metal layer 4 is a copper layer and is 250 nm thick and is located outside the reflection-enhancing layer 3; after calculation, the ratio of the total thickness of the reflection-enhancing structure to the thickness of the corresponding metal layer 4 located on the outer surface of the reflection-enhancing layer 3 is 0.56:1;

[0097] S5. Depositing an anti-oxidation protective layer 5 on the outer surface of the metal layer 4. The thickness of the anti-oxidation protective layer 5 is 30 nm, and the material of the anti-oxidation protective layer 5 is ITO.

[0098] Example 2

[0099] The method of Example 1 is referred to, except that the thickness d2 of the reflection-enhancing layer is adjusted to 60 nm, and it is calculated that d1×n1+d2×n2=D=287 nm.

[0100] Example 3

[0101] The method of Example 1 is referred to, except that the average refractive index n2 of the reflection-enhancing layer between the wavelength of 800nm-1200nm is 1.8, and after calculation, d1×n1+d2×n2=D=272nm. The ratio of n2 to n1 is 0.9:1.

[0102] Example 4

[0103] The method of Example 1 is referred to, except that the opening area of ​​the reflection-enhancing layer is 30% of the area of ​​the corresponding N-type conductive region or P-type conductive region, and the corresponding opening width ratio is the same as the area ratio.

[0104] Example 5

[0105] The method of Example 1 is referred to, except that the material of the reflection enhancement layer is tin oxide. Figure 1 As shown, no opening is provided on the reflection enhancing layer.

[0106] Example 6

[0107] The method of Example 1 is referred to, except that the openings are distributed in a discontinuous point shape, and the corresponding opening area is 10% of the area of ​​the corresponding N-type conductive region or P-type conductive region, and the corresponding opening width ratio is the same as the area ratio.

[0108] Example 7

[0109] The method of Example 1 is referred to, except that the N-type conductive region and the P-type conductive region are a joint passivation structure, the N-type conductive region is a passivation structure of a tunneling oxide layer (with a thickness of 1 nm) and an N-type doped polysilicon layer, and the P-type conductive region is a passivation structure of an intrinsic amorphous silicon layer (with a thickness of 10 nm) and a P-type doped amorphous silicon layer.

[0110] Comparative Example 1

[0111] The method of Example 1 is referred to, except that the reflection enhancing layer is not provided.

[0112] Comparative Example 2

[0113] The method of Example 1 is referred to, except that the thickness d2 of the reflection-enhancing layer is adjusted to 200 nm, and it is calculated that d1×n1+d2×n2=D=490 nm.

[0114] Comparative Example 3

[0115] The method of Example 1 is referred to, except that the average refractive index n2 of the reflection-enhancing layer between the wavelength of 800 nm and 1200 nm is 1.9, and it is calculated that d1×n1+d2×n2=D=276 nm.

[0116] Comparative Example 4

[0117] The method of Example 1 is referred to, except that the average refractive index n2 of the reflection-enhancing layer at a wavelength of 800nm-1200nm is 2.0, which is the same as the average refractive index of the transparent conductive film layer at a wavelength of 800nm-1200nm.

[0118] Test Case

[0119] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.

[0120] Table 1

[0121] Performance Indicators Short circuit current Isc, A Filling factor FF, % Battery conversion efficiency Eff, % Series resistance Rs, Ω Example 1 10.720 0.748 84.63 26.94 Example 2 10.697 0.748 84.66 26.86 Example 3 10.689 0.747 84.50 26.81 Example 4 10.604 0.747 84.41 26.55 Example 5 10.640 0.748 84.12 26.48 Example 6 10.647 0.748 83.83 26.47 Example 7 10.702 0.748 83.85 26.68 Comparative Example 1 10.433 0.747 85.21 26.35 Comparative Example 2 10.494 0.747 84.77 26.41 Comparative Example 3 10.569 0.747 83.71 26.18 Comparative Example 4 10.540 0.747 84.40 26.40

[0122] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can increase the light absorption rate, reduce the free carrier absorption (FCA) of the metal layer to the near-infrared, increase the reflection of the near-infrared band, so as to improve the absorption of the battery substrate to the near-infrared band, thereby improving the short-circuit current of the battery and the battery conversion efficiency.

[0123] Furthermore, according to Example 1 and Examples 2-7, it can be seen that the preferred battery structure of the present invention is more conducive to improving the short-circuit current and battery conversion efficiency of the battery.

[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A back contact cell with a reflection enhancement structure, comprising a cell substrate with a semiconductor distribution layer on the back, and a transparent conductive film layer and a metal layer sequentially arranged on the outer surface of the semiconductor distribution layer, wherein the metal layer covers the transparent conductive film layer, and the semiconductor distribution layer comprises N-type conductive regions and P-type conductive regions arranged alternately, characterized in that: The invention also includes a reflection-enhancing layer disposed between the transparent conductive film layer and the metal layer, wherein the thickness of the corresponding metal layer located on the outer surface of the reflection-enhancing layer is 150-450 nm, the reflection-enhancing layer and the transparent conductive film layer form a reflection-enhancing structure, and the ratio of the total thickness of the reflection-enhancing structure to the thickness of the corresponding metal layer located on the outer surface of the reflection-enhancing layer is 0.3-0.8:1, and the reflection-enhancing structure satisfies: n2 is smaller than n1, the ratio of n2 to n1 is 0.65-0.9:1, n2 is 1.4-1.8, and meets the following corresponding relationship d1×n1+d2×n2=D, the value range of D is 200-300nm; d1 is 40-150nm, n1 is 1.55-2.2, and d2 is 10-150nm; Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm; The material of the reflection enhancement layer is tin oxide and / or zinc oxide; Alternatively, the material of the reflective enhancement layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, and openings are set on the reflective enhancement layer, the openings are distributed in separate points or in continuous lines, and the openings are filled with a metal material corresponding to the metal layer and in contact with the metal layer.

2. The back contact cell with a reflection enhancement structure according to claim 1, characterized in that: The openings of the reflection-enhancing layer are distributed in a continuous linear shape, and the openings are extended along the length direction of the corresponding N-type conductive region or the P-type conductive region.

3. The back contact cell with a reflection enhancement structure according to claim 1, characterized in that: The opening area of ​​the reflection-enhancing layer is 10%-30% of the area of ​​the corresponding N-type conductive region or P-type conductive region.

4. The back contact cell with a reflection enhancement structure according to claim 2 or 3, characterized in that: The openings of the reflection-enhancing layer are composed of a plurality of openings parallel to the N-type conductive region or the P-type conductive region, and the total width of the plurality of openings is 10%-30% of the width of the corresponding N-type conductive region or the P-type conductive region.

5. The back contact cell with a reflection enhancement structure according to claim 1, characterized in that: The back contact cell with a reflection enhancement structure further includes an anti-oxidation protection layer disposed on the outer surface of the metal layer.

6. The back contact cell with a reflection enhancement structure according to claim 1, characterized in that: The material of the metal layer includes at least one of copper, silver, tin and gold.

7. The back contact cell with a reflection enhancement structure according to claim 1, characterized in that: The N-type conductive region includes a first passivation layer and an N-type semiconductor layer, and the P-type conductive region includes a second passivation layer and a P-type semiconductor layer. The first passivation layer and the second passivation layer are independently selected from an intrinsic silicon layer or a tunneling oxide layer.

8. A method for manufacturing a back contact battery, characterized in that: The method is used to prepare a back contact cell provided with a reflection enhancement structure according to any one of claims 1 to 7, and comprises the following steps: S1. Providing a battery substrate with a semiconductor distribution layer on the back side, wherein the semiconductor distribution layer comprises N-type conductive regions and P-type conductive regions arranged alternately; S2, depositing a transparent conductive film layer on the outer surface of the semiconductor distribution layer; S3. Depositing a reflection-enhancing layer on the outer surface of the transparent conductive film layer. The reflection-enhancing layer and the transparent conductive film layer form a reflection-enhancing structure. The reflection-enhancing structure is controlled to meet the following requirements: n2 is smaller than n1 and meets the following corresponding relationship: d1×n1+d2×n2=D, and the value range of D is 200-300nm; Wherein, d1 is the thickness of the transparent conductive film layer, n1 is the average refractive index of the transparent conductive film layer at a wavelength between 800nm ​​and 1200nm, d2 is the thickness of the reflection-enhancing layer, and n2 is the average refractive index of the reflection-enhancing layer at a wavelength between 800nm ​​and 1200nm; S4. Depositing a metal layer on the outer surface of the reflection enhancing layer.

9. The method for manufacturing a back contact battery according to claim 8, characterized in that: The material of the reflective enhancement layer is at least one of silicon oxide, silicon oxynitride, magnesium fluoride, aluminum oxide, and titanium oxide, and the method for manufacturing the back contact battery also includes: after depositing the reflective enhancement layer in S3, the reflective enhancement layer is partially opened, and the openings are distributed in separate points or in continuous lines, and then S4 metal layer is deposited.

10. A photovoltaic module, characterized in that: It comprises a back contact cell with a reflection enhancing structure as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Heterojunction solar cell and preparation method thereof

    CN112151623A

  • Efficient back reflection crystalline silicon heterojunction solar cell and preparation method thereof

    CN113140640A