A non-metal cathode plate for electrolytic manganese dioxide and its preparation method and application

By using a mixture of modified carbon fiber and ultra-fine epoxy resin for warm isostatic pressing and microwave carbonization, combined with CVD surface treatment, a high-performance non-metal cathode plate is prepared, which solves the problem of corrosion resistance of existing cathode plate materials. and the problem of insufficient electrical conductivity, achieving higher electrical conductivity and corrosion resistance.

CN118407076BActive Publication Date: 2024-10-01HUNAN HENGSHENG THERMAL MECHANICAL EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410876036.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

In the current preparation of electrolytic manganese dioxide, the cathode plate material has insufficient corrosion resistance and conductivity, and is easily damaged during transportation and cleaning, resulting in high usage costs.

Method used

A mixture containing graphite powder with different mesh numbers, ultra-fine epoxy resin and surface-modified carbon fiber is used for warm isostatic pressing, followed by microwave carbonization in a microwave sintering furnace, followed by CVD surface treatment to prepare electrolytic dioxide. Non-metallic cathode plates for manganese.

Benefits of technology

It significantly improves the conductivity and corrosion resistance of the cathode plate, reduces the content of copper, iron and other impurities, increases the density and surface smoothness of the cathode plate, avoids the problem of crack bulging, and improves the bending strength and resistivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118407076B_ABST
    Figure CN118407076B_ABST
Patent Text Reader

Abstract

The present invention discloses a non-metal cathode plate for electrolytic manganese dioxide and a preparation method and application thereof, comprising the following steps: mixing raw materials including graphite powder of different mesh sizes, ultrafine epoxy resin and surface modified carbon fiber to obtain a mixture; performing warm isostatic pressing to form the mixture to obtain a green body; placing the green body in a microwave sintering furnace for microwave carbonization, and performing CVD surface treatment on the carbonized plate to obtain the non-metal cathode plate for electrolytic manganese dioxide. The present invention improves the electrical conductivity of the non-metallic carbon-carbon cathode plate, increases the plate density, improves the corrosion resistance and surface smoothness of the plate, and does not produce cracks or bulges on the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolysis, and in particular relates to a non-metal cathode plate for electrolyzing manganese dioxide and a preparation method and application thereof. Background Art

[0002] The main methods for preparing electrolytic manganese dioxide (EMD) include sulfuric acid method, chlorination method, nitric acid method, carbonic acid method and "two-ore method". Among many electrolytic systems, sulfuric acid system has the advantages of low cost, low corrosion and non-toxic gas emission, and is the main medium for preparing EMD. The production method of electrolytic manganese dioxide is as follows: first, manganese carbonate ore is leached with sulfuric acid to obtain manganese sulfate solution, which is then prepared into an electrolyte containing sulfuric acid, and the anode and cathode plates are inserted and energized for electrolytic reaction. At this time, solid manganese dioxide is precipitated on the anode and hydrogen is precipitated on the cathode. The overall reaction formula is:

[0003] MnSO4+2H2O→MnO2+H2SO4+H2↑

[0004] As an essential consumable in the electrolytic manganese dioxide preparation process, the cathode plates currently on the market are mainly copper cathode plates, graphite cathode plates, and carbon-carbon cathode plates.

[0005] Since copper materials are not corrosion-resistant and are expensive, and will introduce copper impurities into the product during electrolysis, cathode plates made of carbon materials are superior to copper materials in overall parameters and have more advantages in EMD mass production.

[0006] Graphite cathode plates are highly brittle and easily damaged during transportation, cleaning and other maintenance processes. They need to be replaced frequently, which greatly increases their cost of use.

[0007] The carbon-carbon cathode plate with added carbon fiber reinforcement has strong impact toughness and can effectively solve the loss problem during maintenance. However, its resistivity and corrosion resistance are lower than those of the graphite cathode, and cracks and bulging are prone to occur on the surface during the sintering process, and the surface smoothness is poor. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a non-metallic cathode plate for electrolyzing manganese dioxide and a preparation method and application thereof.

[0009] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0010] A method for preparing a non-metallic cathode plate for electrolytic manganese dioxide comprises the following steps:

[0011] (1) mixing raw materials including graphite powder of different mesh sizes, ultrafine epoxy resin and surface-modified carbon fiber to obtain a mixture; the surface-modified carbon fiber is obtained by subjecting the carbon fiber to oxygen oxidation treatment at a treatment temperature of 150-200° C.;

[0012] (2) forming the mixed material by warm isostatic pressing to obtain a green body;

[0013] (3) Placing the green body in a microwave sintering furnace for microwave carbonization, and subjecting the carbonized electrode plate to CVD surface treatment to obtain the non-metallic cathode plate for electrolytic manganese dioxide; the microwave carbonization is carried out by microwave heating under a protective atmosphere, and the temperature is increased in a step-like manner to 950-1050° C. at a set heating rate, and then cooled at a set cooling rate.

[0014] As a further improvement, the graphite powder in step (1) includes graphite powder of 300-350 mesh, 650-900 mesh and 1100-1300 mesh, with a mass ratio of 20-30:10-30:50.

[0015] As a further improvement, the ultrafine epoxy resin particle size D50 in step (1) is 5 to 15 microns.

[0016] As a further improvement, the carbon fiber in step (1) is chopped fiber, and the length of the chopped fiber is 2-7 mm.

[0017] As a further improvement, the mass ratio of the graphite powder of different mesh sizes, the ultrafine epoxy resin, and the surface modified carbon fiber in step (1) is 65~78:25~18:10~4.

[0018] As a further improvement, the warm isostatic pressing in step (2) controls the pressing temperature to be 120-150° C. and the pressing pressure to be 100-300 MPa.

[0019] As a further improvement, the microwave carbonization process in step (3) is as follows: heating to 150-170°C for 0.5-1h and keeping warm for 10-30min, heating to 220-300°C for 2-3h and keeping warm for 1.5-2h, heating to 350-400°C for 10-16h and keeping warm for 10-30min, heating to 580-620°C for 40-80h and keeping warm for 4-6h, heating to 840-860°C for 10-16h and keeping warm for 5-8h, heating to 950-1050°C for 8-10h and keeping warm for 4-6h, then cooling to 580-620°C for 6-10h and keeping warm for 1-2h, cooling to 390-430°C for 4-6h, keeping warm for 2-4h and then naturally cooling to room temperature.

[0020] As a further improvement, the CVD surface treatment in step (3) uses a carbon source gas for chemical vapor deposition.

[0021] The invention also provides a non-metal cathode plate for electrolyzing manganese dioxide obtained by the preparation method.

[0022] The present invention also provides an application of the non-metal cathode plate in the preparation of electrolytic manganese dioxide.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] Compared with copper cathode, the non-metal cathode plate material for electrolytic manganese dioxide of the present invention has greatly improved electrocatalytic effect and conductivity, significantly reduced impurities such as copper and iron in the product, and has a smaller specific surface area and a more rigorous microstructure.

[0025] Based on the current carbon-carbon cathode plate, the present invention further improves the conductivity of the non-metallic carbon-carbon cathode plate by improving the formula and preparation process, increases the plate density, improves the corrosion resistance and surface smoothness of the plate, and no cracks or bulges will occur on the surface.

[0026] The surface density of the cathode plate prepared by the present invention is 1.75-1.85 g / cm 3 The flexural strength is 65~85Mpa and the resistivity is 15~18 microohm-meters. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 1 is the cathode polarization curve of Example 1 of the present invention and three materials of Cu and graphite;

[0029] Figure 2 The microscopic morphology SEM analysis of the manganese dioxide products prepared from three different cathode materials, Cu and graphite, in Example 1 of the present invention;

[0030] Figure 3 This is the finished cathode plate prepared in Example 1. DETAILED DESCRIPTION

[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0032] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0034] In some specific embodiments of the present invention, the method for preparing a non-metallic cathode plate for electrolytic manganese dioxide comprises the following steps:

[0035] (1) Raw materials including graphite powder of different mesh sizes, ultrafine epoxy resin and surface-modified carbon fiber are mixed to obtain a mixture.

[0036] In some embodiments, the graphite powder includes graphite powder of 300-350 mesh, 650-900 mesh and 1100-1300 mesh, preferably in a mass ratio of 20-30:10-30:50. In some preferred embodiments, the graphite powder is graded 325 mesh: 800 mesh: 1250 mesh in a ratio of 20-30:10-30:50. Preferably, the purity of the graphite powder is 95%-99%. The graphite powder particles of different mesh sizes are graded, the fine powder increases the density of the pressed embryo, and the coarse powder relieves the residual stress in the embryo to prevent cracking during carbonization and sintering.

[0037] In some embodiments, the ultrafine epoxy resin particle size D50 is 5 to 15 microns. The adhesive molding agent uses ultrafine epoxy resin, which has low softening point and curing point (80 to 90°C and 120 to 130°C, respectively). The heating temperature required during the pressing process is low, which saves energy and increases efficiency. At the same time, the curing shrinkage of epoxy resin is 1 to 2%, while that of phenolic resin is 8 to 10%. Ultrafine epoxy resin can better embed into the gaps of fiber bundles, and also prevent the fibers from agglomerating with coarse particles as the core and being difficult to disperse. Better dispersion effect can reduce the internal stress caused by uneven composition inside the embryo, reduce internal defects during sintering, and better dispersion effect will also improve the conductivity and bending strength of the product.

[0038] In some embodiments, the carbon fiber is chopped fiber, and the length of the chopped fiber is 2-7 mm. The surface-modified carbon fiber is subjected to oxygen oxidation treatment before mixing, and the treatment temperature is preferably 150-200° C. for 1-3 hours. The surface oxidation modification of the carbon fiber enhances the dispersibility and the bonding with the resin, and improves the flexural strength of the product.

[0039] In some embodiments, the mass ratio of the graphite powder of different mesh sizes, the ultrafine epoxy resin, and the surface modified carbon fiber is 65~78:25~18:10~4.

[0040] In some embodiments, the mixing is to first mix graphite powders of different gradations and ultrafine epoxy resin for 1 to 2 hours, and then add the surface modified carbon fiber into the mixture and continue mixing for 1 to 3 hours.

[0041] (2) The mixed material is subjected to warm isostatic pressing to obtain a green body.

[0042] In some embodiments, the mixed material is first molded, and then the molded powder is pressed by warm isostatic pressing. Preferably, the pressing temperature of the warm isostatic pressing is controlled to be 120-150° C. and the pressing pressure is 100-300 MPa.

[0043] Molding adopts compression molding and isostatic pressing to further enhance the density of the embryo, ensure uniform density of the embryo, reduce internal defects of the embryo, improve the uniformity of the resistivity of the finished product, and achieve better conductive performance.

[0044] (3) Placing the green body in a microwave sintering furnace for microwave carbonization, and subjecting the carbonized electrode plate to CVD surface treatment to obtain the non-metallic cathode plate for electrolytic manganese dioxide.

[0045] In some embodiments, the process of microwave carbonization treatment is: under a protective atmosphere (such as nitrogen), the temperature is raised to 150-170°C for 0.5-1h and kept warm for 10-30min, the temperature is raised to 220-300°C for 2-3h and kept warm for 1.5-2h, the temperature is raised to 350-400°C for 10-16h and kept warm for 10-30min, the temperature is raised to 580-620°C for 40-80h and kept warm for 4-6h, the temperature is raised to 840-860°C for 10-16h and kept warm for 5-8h, the temperature is raised to 950-1050°C for 8-10h and kept warm for 4-6h, then the temperature is lowered to 580-620°C for 6-10h and kept warm for 1-2h, and then the temperature is lowered to 390-430°C for 4-6h, and naturally cooled to room temperature (20-25°C) after keeping warm for 2-4h. Maintain a slight positive pressure of 2~10Kpa during the cooling process.

[0046] The present invention adopts a specific heating curve, the temperature rises in a step-like manner and the heating rate and cooling rate need to be controlled. The heating rate is slowed down in the temperature section where the epoxy resin loses weight faster to ensure that a large amount of gas is not generated. Since the embryo is dense and the exhaust is slow, a large amount of gas generated in a short period of time will cause cracks and bulges inside and on the surface of the embryo. Controlling the cooling rate is to prevent the rapid cooling from causing a large temperature difference between the surface and the inside of the embryo, and the different thermal expansions cause large shear stresses on the surface and inner layer, and finally cracks on the embryo surface.

[0047] Microwave heating is used in the carbonization stage to evenly heat the inside and outside, avoiding the difficulty of escaping the internal gas and molding agent of the embryo body caused by the traditional heating method, and the defects of blistering on the surface of the sintered product. At the same time, it also reduces the generation of internal microcracks and improves the strength and conductivity of the embryo body. The molding agent can be collected by serpentine filter disc, alumina ceramic adsorption condensation and stainless steel filter adsorption.

[0048] In some embodiments, the CVD surface treatment uses a carbon source gas for chemical vapor deposition, such as a single carbon source gas or a mixed gas of hydrocarbons such as methane, acetylene, and propane. In some embodiments, the process of the CVD surface treatment is as follows: place the electrode plate in a chemical vapor deposition furnace, evacuate to the limit, maintain the pressure for 15 to 30 minutes, ensure that the pressure rise rate is ≤15pa / min, heat to 950 to 1100°C, turn on the vacuum pump again and introduce the carbon source gas to start deposition, and the nitrogen ventilation volume of the outer chamber of the deposition furnace is 2 to 6m 3 / h, carbon source gas ventilation volume 40~80m 3 / h, the vacuum degree is maintained at 3.5~5Kpa.

[0049] The surface chemical vapor deposition of the cathode plate further increases the surface density and smoothness, reduces the adhesion of Ca and Mg crystals, and at the same time, the densified plate has better impact strength and corrosion resistance.

[0050] Example 1

[0051] The method for preparing the non-metallic cathode plate of this embodiment includes the following steps:

[0052] (1) Raw materials including graphite powder of different mesh sizes (325 mesh: 800 mesh: 1250 mesh in a ratio of 30:20:50, graphite powder purity 99%), ultrafine epoxy resin (D50 = 15 μm) and surface modified carbon fiber were mixed in a mass ratio of 65:25:10. The graphite powder and ultrafine epoxy resin were first mixed for 1 h, and then the surface modified carbon fiber was added and mixed for 2 h to obtain a mixture.

[0053] Among them, the preparation method of surface modified carbon fiber is as follows: the carbon fiber (short-cut fiber with a length of 3 mm) is subjected to oxygen oxidation treatment at a treatment temperature of 150° C. for 2 hours.

[0054] (2) The mixed material is first molded, and then the molded powder is pressed by warm isostatic pressing (pressing temperature is 130°C, pressing pressure is 150 MPa) to obtain a green body.

[0055] (3) The green body is placed in a microwave sintering furnace for microwave carbonization, and the electrode plate after carbonization is subjected to CVD surface treatment to obtain a non-metallic cathode plate.

[0056] Among them, the process of microwave carbonization treatment is: under a protective atmosphere, the temperature is raised to 150°C for 1 hour and kept warm for 30 minutes, the temperature is raised to 220°C for 2 hours and kept warm for 2 hours, the temperature is raised to 400°C for 15 hours and kept warm for 30 minutes, the temperature is raised to 600°C for 70 hours and kept warm for 4 hours, the temperature is raised to 850°C for 15 hours and kept warm for 5 hours, the temperature is raised to 1000°C for 10 hours and kept warm for 4 hours, then the temperature is lowered to 600°C for 10 hours and kept warm for 2 hours, and then the temperature is lowered to 400°C for 6 hours and kept warm for 3 hours before naturally cooling to room temperature. During the cooling process, pay attention to maintaining a slight positive pressure of 10Kpa.

[0057] The process of CVD surface treatment is as follows: place the plate in a chemical vapor deposition furnace, evacuate to the limit, maintain pressure for 30 minutes, ensure that the pressure rise rate is ≤15pa / min, heat to 1060℃, turn on the vacuum pump again and introduce carbon source gas (methane) to start deposition, and the nitrogen ventilation volume of the outer chamber of the deposition furnace is 6m 3 / h, carbon source gas ventilation volume 60m 3 / h, the vacuum degree is maintained at 5Kpa.

[0058] The cathode plate product prepared in this embodiment is as follows Figure 3 , smooth surface, no cracks or bulges, surface density 1.75g / cm 3 The flexural strength (according to GB / T 3074.1-2021) is 65Mpa and the resistivity is 17 microohm-meter.

[0059] Comparative Example 1

[0060] Compared with Example 1, the only difference of this comparative example is that the graphite powder in step (1) uses only one mesh size (800 mesh). The other steps and parameters are the same as those in Example 1.

[0061] The surface density of the cathode plate prepared in this comparative example is 1.60 g / cm 3 , flexural strength is 60Mpa and resistivity is 22 microohms.

[0062] Comparative Example 2

[0063] Compared with Example 1, the only difference of this comparative example is that phenolic resin is used in step (1) to replace the ultrafine epoxy resin. The other steps and parameters are the same as those of Example 1.

[0064] The surface density of the cathode plate prepared in this comparative example is 1.65 / cm 3 , flexural strength is 55Mpa and resistivity is 25 microohm-meters.

[0065] Comparative Example 3

[0066] Compared with Example 1, the only difference of this comparative example is that the carbon fiber in step (1) is not subjected to oxygen oxidation treatment. The other steps and parameters are the same as those in Example 1.

[0067] The surface density of the cathode plate prepared in this comparative example is 1.7 g / cm 3 , flexural strength is 50Mpa and resistivity is 20 microohm-meter.

[0068] Comparative Example 4

[0069] Compared with Example 1, the only difference of this comparative example is that the process of microwave carbonization treatment in step (3) is: carbonization is carried out using a graphite heating element carbonization furnace.

[0070] The other steps and parameters are the same as those in Example 1.

[0071] The surface density of the cathode plate prepared in this comparative example is 1.7 g / cm 3 , flexural strength is 60Mpa and resistivity is 20 microohm-meter.

[0072] Comparative Example 5

[0073] Compared with Example 1, the only difference of this comparative example is that the process of microwave carbonization treatment in step (3) is as follows: heating to 220°C for 2 h and keeping warm for 30 min, heating to 400°C for 10 h and keeping warm for 30 min, heating to 600°C for 40 h and keeping warm for 4 h, heating to 850°C for 10 h and keeping warm for 5 h, heating to 950°C for 5 h and keeping warm for 4 h, then cooling to 600°C for 2 h and keeping warm for 2 h, cooling to 400°C for 4 h and keeping warm for 3 h, and then naturally cooling to room temperature. During the cooling process, pay attention to maintaining a slight positive pressure of 10 Kpa.

[0074] The other steps and parameters are the same as those in Example 1.

[0075] The surface density of the cathode plate prepared in this comparative example is 1.7 g / cm 3 , flexural strength is 45Mpa and resistivity is 30 microohm-meter.

[0076] Electrolytic manganese dioxide experiment

[0077] Solution system: MnSO4 (50 g / L) + H2SO4 (45 g / L);

[0078] Electrolysis temperature: 98°C;

[0079] Current density: 80A / m 2 ;

[0080] Anode material: TA1 titanium plate;

[0081] Cathode materials: cathode plate prepared in Example 1, copper cathode, isostatic graphite;

[0082] Running time: 300h.

[0083] Figure 1 is the cathode polarization curve of Example 1 and three materials of Cu and graphite. Figure 1 It can be seen that the current of the graphite and the cathode plates of Example 1 tends to be stable with the increase of potential, and there is no obvious polarization phenomenon, while the current of the copper electrode rises sharply with the increase of potential, and obvious polarization phenomenon occurs.

[0084] Figure 2 The SEM analysis of the microscopic morphology of the manganese dioxide products prepared by three different cathode materials, Cu and graphite, in Example 1. Among them, the microscopic morphology of the manganese dioxide electrolyzed by copper cathode: (a1) the morphology of the manganese dioxide product after 80 hours; (a2) the morphology of the manganese dioxide product after 160 hours; (a3) ​​the morphology of the manganese dioxide product after 240 hours; it can be seen from the figure that after 240 hours, more dense calcium and magnesium crystals are produced on the surface of the copper cathode plate, and the dendrites are obvious.

[0085] Microstructure of manganese dioxide electrolyzed by graphite cathode: (b1) morphology of manganese dioxide product at 80h; (b2) morphology of manganese dioxide product at 160h; (b3) morphology of manganese dioxide product at 240h; indicating that there is shallow calcium and magnesium crystal deposition on the surface of graphite cathode at 240h, and dendrites do not grow over a large area.

[0086] The microscopic morphology of manganese dioxide electrolyzed at the cathode of Example 1: (c1) morphology of the manganese dioxide product at 80h; (c2) morphology of the manganese dioxide product at 160h; (c3) morphology of the manganese dioxide product at 240h; it shows that the surface morphology of the carbon-carbon cathode of Example 1 has not changed significantly after 240h, and there is no calcium and magnesium crystals attached to the surface.

[0087] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a non-metallic cathode plate for electrolytic manganese dioxide, characterized in that: The steps include: (1) mixing raw materials including graphite powder of different mesh sizes, ultrafine epoxy resin and surface-modified carbon fiber to obtain a mixture; the surface-modified carbon fiber is obtained by subjecting the carbon fiber to oxygen oxidation treatment at a treatment temperature of 150-200° C.; The graphite powder includes 300-350 mesh, 650-900 mesh and 1100-1300 mesh graphite powder, with a mass ratio of 20-30:10-30:50; the ultrafine epoxy resin particle size D50 is 5-15 microns; (2) forming the mixed material by warm isostatic pressing to obtain a green body; (3) placing the green body in a microwave sintering furnace for microwave carbonization, and performing CVD surface treatment on the carbonized electrode plate to obtain the non-metallic cathode plate for electrolytic manganese dioxide; the microwave carbonization is performed by microwave heating under a protective atmosphere; The microwave carbonization process is as follows: heating to 150-170°C for 0.5-1h and keeping the temperature for 10-30min, heating to 220-300°C for 2-3h and keeping the temperature for 1.5-2h, heating to 350-400°C for 10-16h and keeping the temperature for 10-30min, heating to 580-620°C for 40-80h and keeping the temperature for 4-6h, heating to 840-860°C for 10-16h and keeping the temperature for 5-8h, heating to 950-1050°C for 8-10h and keeping the temperature for 4-6h, then cooling to 580-620°C for 6-10h and keeping the temperature for 1-2h, cooling to 390-430°C for 4-6h, keeping the temperature for 2-4h and then cooling naturally to room temperature.

2. The method for preparing a non-metallic cathode plate for electrolytic manganese dioxide according to claim 1, characterized in that: The carbon fiber in step (1) is chopped fiber, and the length of the chopped fiber is 2-7 mm.

3. The method for preparing a non-metallic cathode plate for electrolytic manganese dioxide according to claim 1, characterized in that: The mass ratio of the graphite powder of different mesh sizes, the ultrafine epoxy resin, and the surface modified carbon fiber in step (1) is 65-78:25-18:10-4.

4. The method for preparing a non-metallic cathode plate for electrolytic manganese dioxide according to claim 1, characterized in that: In step (2), the warm isostatic pressing controls the pressing temperature to be 120-150° C. and the pressing pressure to be 100-300 MPa.

5. The method for preparing a non-metallic cathode plate for electrolytic manganese dioxide according to claim 1, characterized in that: The CVD surface treatment in step (3) uses a carbon source gas for chemical vapor deposition.

6. A non-metallic cathode plate for electrolytic manganese dioxide obtained by the preparation method according to any one of claims 1 to 5.

7. Use of the non-metallic cathode plate according to claim 6 in the preparation of electrolytic manganese dioxide.