A plug-and-play micro-nano spray needle manufacturing method and micro-nano spray needle
Silicon nanoconcave molds are prepared by oxygen plasma treatment and angle molding peeling method, and PDMS nanoconvex molds are manufactured by combining the casting method, which realizes the sealing and bonding of polymer micro-nano spray needles and solves the problems of spray needle clogging and difficult size control. , improving printing efficiency and convenience.
Patent Information
- Application Number
- CN202410882695.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-03
AI Technical Summary
Existing micro-nano spray needles are prone to clogging due to debris, particles and chemical reaction products during the printing process, and their size control and repeatability are low, making it difficult to achieve efficient plug-and-play manufacturing.
A PDMS spray needle cover plate and an unbonded polymer micro-nano spray needle were used for oxygen plasma treatment, and a silicon nano concave mold was prepared by the angle forming and peeling method. The PDMS nano convex mold was obtained by the casting method to form micron channels and steel needle preforms. The connecting channel is left to realize the sealing and bonding of the polymer micro-nano spray needle.
It improves the plug-and-playability of micro-nano spray needles, enhances printing efficiency and ease of use, and solves the problems of spray needle clogging and difficult size control.
Smart Images

Figure CN118418349B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of micro-electromechanical technology, and in particular to a plug-and-play micro-nano spray needle manufacturing method and the micro-nano spray needle. Background Art
[0002] Electrohydraulic jet is a technology that can directly print micro-nano patterns using solution ink. Additive manufacturing can be performed on demand, and various functional materials can be directly printed on the target substrate to achieve low-cost direct writing of high-resolution micro-nano patterns. It is used in the fields of flexible electronic device manufacturing, biochemical printing, field effect transistors and organic light-emitting diodes. Studies have shown that electrohydraulic jet has a scale effect, and reducing the inner diameter of the needle is an effective way to achieve nanoscale printing. However, during the printing process, the micro-nano needle is easily clogged by the accumulation, adhesion or deterioration of debris, particulate matter, sediments, chemical reaction products, etc., which makes the needle a consumable in the printing process. Therefore, how to manufacture plug-and-play micro-nano needles on a large scale is a major problem that needs to be solved urgently in this field.
[0003] At present, a quartz needle with a size of 300nm can be obtained by heating and stretching with a Sutter drawing instrument, but the size is difficult to control during the heating and stretching process and it is very easy to break. The preparation of micro-nano needles using nanocracks caused by thermal shrinkage and volume shrinkage due to stress release after SU-8 photoresist development can obtain polymer SU-8 needles with a size of 250nm, but this method also has problems such as difficult control and low repeatability. Summary of the invention
[0004] The present invention overcomes the deficiencies of the prior art and provides a plug-and-play micro-nano spray needle manufacturing method and a micro-nano spray needle, which has a simple manufacturing process and achieves a plug-and-play use effect of the micro-nano spray needle, greatly improving printing efficiency and convenience of use.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a plug-and-play micro-nano spray needle manufacturing method, comprising the following steps:
[0006] Step S1. treating the PDMS needle cover plate and the unbonded polymer micro-nano needle with oxygen plasma;
[0007] The preparation method of the unbonded polymer micro-nano spray needle comprises:
[0008] Step a.1. Prepare a silicon nanoconcave mold by using an angle molding peeling method;
[0009] Step a.2. Using the silicon nano-concave mold prepared in step a.1, a PDMS nano-convex mold is obtained by casting, and the PDMS nano-convex mold has nano-ridges;
[0010] Step a.3. Print a plurality of convex lines extending outward from one side of the nano-ridge of the PDMS nano-convex mold prepared in step a.2, print a plurality of convex lines to form a micron channel convex mold on the PDMS nano-convex mold, and a steel needle reserved connection channel convex mold connected to the micron channel; obtain a PDMS-PEO micro-nano spray needle convex mold;
[0011] Step a.4. Using the PDMS-PEO micro-nano spray needle convex mold prepared in step a.3, an unbonded polymer micro-nano spray needle is obtained by casting, wherein the unbonded polymer micro-nano spray needle has a reserved connection channel for a microchannel steel needle;
[0012] The preparation method of the PDMS needle cover plate comprises:
[0013] Step b.1. obtaining a glass substrate, performing a hydrophilic treatment on the glass substrate, and printing a convex line on the hydrophilic treated glass substrate;
[0014] Step b.2. Pour the PDMS mixed solution onto the glass substrate, and place it in an oven at 60-85°C for 2-4 hours for curing. After cooling to room temperature, separate it from the glass substrate to obtain a PDMS needle cover with a reserved channel for the steel needle.
[0015] Step S2. Then aligning and bonding the PDMS needle cover plate with the reserved channel of the steel needle with the unbonded polymer micro-nano needle to seal the micro-nano channel of the needle and obtain the polymer micro-nano needle;
[0016] Step S3: insert the hydrophilic treated steel needle into the reserved connection channel of the polymer micro-nano spray needle for interference fit.
[0017] In a preferred embodiment of the present invention, the angle forming peeling method is used to prepare the silicon nano concave mold, comprising the following steps:
[0018] Step a.1.1. Place the silicon wafer with the silicon dioxide layer as a mold blank in a drying tower filled with hexamethyldisilazane atmosphere for 10 to 20 minutes to enhance the adhesion between the silicon dioxide layer and the photoresist;
[0019] Step a.1.2. Then, a layer of photoresist is spin-coated on the outer surface of the silicon dioxide layer of the mold blank treated in step a.1.1; in step a.1.2, the spin coating parameters of the photoresist are: low speed 600~900rpm, spin coating time 6~9s, high speed 6000~9000rpm, spin coating time 20~30s;
[0020] Step a.1.3. Place the mold blank processed in step a.1.2 on a hot plate for pre-baking and then UV exposure;
[0021] Step a.1.4. Place the mold blank treated in step a.1.3 on a hot plate at 100-120°C and reverse bake for 1-3 minutes; after cooling to room temperature, perform full exposure for 60-80 seconds, and after developing for 40-60 seconds, form a micron-scale inverted trapezoidal photoresist step on the mold blank;
[0022] Step a.1.5. The mold blank with the micron-scale inverted trapezoidal photoresist step processed in step a.1.4 is etched with a hydrofluoric acid buffer solution for 8 to 15 seconds to etch away the silicon dioxide layer except for the bottom of the photoresist; then a layer of copper film is vertically deposited directly above the photoresist of the mold blank, and a nano-gap is generated between the silicon dioxide layer below the micron-scale inverted trapezoidal photoresist step and the deposited copper film;
[0023] Step a.1.6. Soak the mold blank treated in step a.1.5 in an acetone solution for 30 to 60 minutes, then peel off and remove the photoresist, leaving a nano-gap between the silicon dioxide layer on the mold blank and the deposited copper film;
[0024] Step a.1.7. The mold blank processed in step a.1.6 is etched using a reactive ion deep etching technique to etch the exposed silicon wafer, thereby forming a nanochannel on the silicon wafer;
[0025] Step a.1.8. Use hydrofluoric acid buffer to remove the remaining silicon dioxide layer from the mold blank treated in step a.1.7, and use concentrated nitric acid to remove the copper film to obtain a silicon nano-concave mold.
[0026] In a preferred embodiment of the present invention, a PDMS nanoconvex mold is manufactured by a casting method, comprising the following steps:
[0027] Step a.2.1. Place the silicon nanoconcave mold in dimethyldichlorosilane, toluene and ethanol solutions respectively and soak for 15 to 30 seconds to form an anti-adhesive layer;
[0028] Step a.2.2. Pour the PDMS mixed solution onto the silicon nano-concave mold, place it in a vacuum environment with a vacuum degree of less than 10Pa for at least 1 hour, so that the PDMS mixed solution completely fills the silicon nano-concave mold, and then place it in a 60~85℃ oven and bake it for 2~4 hours to solidify. After cooling to room temperature; separate the PDMS nano-convex mold formed by the solidified PDMS mixed solution from the silicon nano-concave mold to obtain the PDMS nano-convex mold.
[0029] In a preferred embodiment of the present invention, the step of preparing the PDMS-PEO micro-nano spray needle convex mold further includes:
[0030] Step a.3.1. The PDMS nanoconvex mold is treated with oxygen plasma at a treatment power of 5 to 20 W and a treatment time of 10 to 30 seconds. In order to improve the bonding force between the printing material and the PDMS nanoconvex mold, the PDMS nanoconvex mold is treated with oxygen plasma before electrojet printing.
[0031] Step a.3.2. Print the micron channel convex mold and the steel needle reserved connection channel convex mold on the PDMS nanoconvex mold after oxygen plasma treatment.
[0032] In a preferred embodiment of the present invention, in step S1, the treatment power of the oxygen plasma treatment is 5-20 W, and the treatment time is 10-30 s;
[0033] and\or, in step a.4, the depth of the micron channel is greater than the depth of the nano channel, and the micron channel is combined to form a step-by-step gradually narrowing path extending from the micron channel to the nano needle tip of the polymer micro-nano spray needle;
[0034] and\or, the convex line in step b.1 is a 50 mm convex line;
[0035] and\or, in step b.2, the volume ratio of the PDMS mixed solution is 4:1 to 10:1 of PDMS and curing agent;
[0036] and\or, in step S3, one end of the steel needle is inserted into the steel needle reserved connection channel of the polymer micro-nano spray needle and communicated with the microchannel, and the other end of the steel needle is located outside the polymer micro-nano spray needle;
[0037] And\or, in step a.3.2, the method for printing a plurality of convex lines includes:
[0038] Print a 50mm wide convex line with the parameters of voltage 1500~2200V, concentration 1~3wt% PEO, and working distance 500~700mm as a microchannel convex mold; extend and print a 100mm wide convex line on the basis of the 50mm line, with the parameters of voltage 2000~2500V, concentration 2~4wt% PEO, and working distance 600~800mm as a microchannel convex mold; then extend and print another 50mm convex line on the basis of the 100mm line as a steel needle reserved connection channel convex mold;
[0039] And\or, in step a.1.3, the hot plate pre-baking is to place the silicon wafer spin-coated with the photoresist on a 100-120°C hot plate for pre-baking for 1-3 minutes; the UV exposure exposure time is 2-15 seconds;
[0040] In step a.2.2, the volume ratio of the PDMS mixed solution is 4:1 to 10:1.
[0041] In a preferred embodiment of the present invention, the method of casting the PDMS-PEO micro-nano spray needle convex mold to obtain the unbonded polymer micro-nano spray needle comprises:
[0042] Step a.4.1. Place the PDMS-PEO micro-nano spray needle convex mold in a drying tower filled with trimethylchlorosilane atmosphere and let it stand for 5 to 20 minutes;
[0043] Step a.4.2. Pour the mixed PDMS solution onto the PDMS-PEO micro-nano spray needle convex mold, and place it in a vacuum oven to evacuate for 1-2 hours to ensure that the PDMS mixed solution completely fills the PDMS-PEO micro-nano spray needle convex mold;
[0044] Step a.4.3. Place the PDMS-PEO micro-nano spray needle convex mold cast with the PDMS mixed solution in a 60~85℃ oven and bake for 2~4 hours to solidify. After cooling to room temperature, separate the unbonded polymer micro-nano spray needle formed after the PDMS mixed solution is solidified from the mold to obtain an unbonded polymer micro-nano spray needle.
[0045] In a preferred embodiment of the present invention, the photoresist is AZ701, AZ703, AZ5214E, AR-N4240, AR-N4340, AR-P5300, AR-N4400, AR-U4000, BP212, BN308, NR26-8000P, PR1-1500A1, or SU-8 photoresist;
[0046] And / or, the copper film can be replaced by Al, Cr, Au, Ag, SiO2 or Ni; and the nitric acid can be replaced by aqua regia.
[0047] In a preferred embodiment of the present invention, in step b.2, the volume ratio of the PDMS mixed solution is 4:1-10:1; the curing temperature is 60°-85°C, and the curing time is 2-4h;
[0048] And / or, in step b.1, convex lines are printed, the printing voltage is controlled at 1500~2100V, the material used is PEO printing material or PVP printing material, the PEO concentration of PEO printing material is 1~3wt%; the PVP concentration of PVP printing material is 1~5wt%; the convex lines printed in step b.1 are subjected to atmosphere treatment with trimethylchlorosilane for 5~20min.
[0049] In a preferred embodiment of the present invention, after step S3, step S4 is further included to trim the shape of the polymer micro-nano spray needle processed in step S3. The trimming includes cutting off excess PDMS material to obtain the needle contour, thereby obtaining a plug-and-play micro-nano spray needle.
[0050] In a preferred embodiment of the present invention, a micro-nano spray needle is prepared by using the plug-and-play micro-nano spray needle manufacturing method.
[0051] The present invention solves the defects existing in the technical background, and the beneficial technical effects of the present invention are:
[0052] The plug-and-play micro-nano spray needle manufacturing method and the micro-nano spray needle of the present invention have simple manufacturing process, achieve the plug-and-play use effect of the micro-nano spray needle, and greatly improve the printing efficiency and convenience of use.
[0053] The invention replicates the nano pattern on the silicon nano concave mold by a casting method to obtain a PDMS nano convex mold, and manufactures a nozzle micron channel convex mold by printing lines to form a PDMS-PEO micro-nano nozzle convex mold; PDMS is used to cast the PDMS-PEO micro-nano nozzle convex mold to obtain an unbonded polymer micro-nano nozzle, and an oxygen plasma treatment method is used to bond the unbonded polymer micro-nano nozzle and the PDMS nozzle cover plate to seal the nozzle micro-nano channel to obtain a complete polymer micro-nano nozzle. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0055] Figure 1 It is a flow chart of manufacturing a silicon nano-concave mold according to a preferred embodiment of the present invention.
[0056] Figure 2 It is a manufacturing flow chart of a PDMS nanoconvex mold in the plug-and-play micro-nano spray needle manufacturing process of a preferred embodiment of the present invention.
[0057] Figure 3 It is a manufacturing flow chart of a PDMS-PEO micro-nano spray needle convex mold and an unbonded polymer micro-nano spray needle in the plug-and-play micro-nano spray needle manufacturing process of a preferred embodiment of the present invention.
[0058] Figure 4 It is a schematic structural diagram of the bonding of an unbonded polymer micro-nano spray needle and a PDMS spray needle cover plate in the plug-and-play micro-nano spray needle manufacturing process of a preferred embodiment of the present invention.
[0059] Figure 5 It is a schematic structural diagram of the plug-and-play micro-nano spray needle in the preferred embodiment of the present invention, in which the unbonded polymer micro-nano spray needle and the PDMS spray needle cover plate are bonded and then the steel needle is inserted.
[0060] Figure 6 It is a schematic diagram of the plug-and-play micro-nano spray needle structure of a preferred embodiment of the present invention.
[0061] Figure 7 1 is a scanning electron microscope image of a silicon nanoconcave mold according to a preferred embodiment of the present invention.
[0062] Figure 8 This is a scanning electron microscope image of a plug-and-play micro-nano spray needle according to a preferred embodiment of the present invention.
[0063] Fig. 9 This is an atomic force microscope image of the nano-ridge disconnection phenomenon on the PDMS nano-convex mold of the preferred embodiment of the present invention.
[0064] In the figure: 1. Silicon wafer; 2. Silicon dioxide layer; 3. Photoresist; 4. Photolithography mask; 5. Ultraviolet light; 6. Copper film; 7. Silicon nano-concave mold; 8. PDMS mixed solution; 9. PEO material; 10. Steel needle. DETAILED DESCRIPTION
[0065] The present invention will now be further described in detail with reference to the accompanying drawings and embodiments. These drawings are simplified schematic diagrams that only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0066] It should be noted that if there are directional indications (such as up, down, bottom, top, etc.) involved in the embodiments of the present invention, the directional indication is only used to explain the relative position relationship, movement, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly. The terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Unless otherwise clearly specified and defined, the terms "set", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. Embodiment 1
[0067] like Figure 1-Figure 9 As shown, in order to achieve the above purpose, the technical solution adopted by the present invention is: a plug-and-play micro-nano spray needle manufacturing method, comprising the following steps:
[0068] Step S1. The PDMS spray needle cover plate and the unbonded polymer micro-nano spray needle are subjected to oxygen plasma treatment. The treatment power of the oxygen plasma treatment is 5-20 W, and the treatment time is 10-30 s.
[0069] Step S2. Then, the steel needle reserved channel of the PDMS needle cover is aligned and bonded with the steel needle reserved connection channel on the unbonded polymer micro-nano needle to seal the micro-nano channel of the needle and obtain the polymer micro-nano needle (such as Figure 4 shown);
[0070] Step S3. Insert the hydrophilic treated steel needle 10 into the reserved connection channel of the polymer micro-nano spray needle for interference fit. One end of the steel needle 10 is inserted into the reserved connection channel of the polymer micro-nano spray needle and communicated with the microchannel, and the other end of the steel needle 10 is located outside the polymer micro-nano spray needle.
[0071] Specifically, the preparation method of the unbonded polymer micro-nano spray needle (such as Figure 1 , Figure 2 shown) include:
[0072] Step a.1. Prepare the silicon nano-concave mold 7 (such as Figure 1 shown);
[0073] Furthermore, the silicon nano-concave mold 7 is prepared by an angle molding peeling method, which includes the following steps:
[0074] Step a.1.1. Place the silicon wafer 1 with the silicon dioxide layer 2 as a mold blank in a drying tower filled with hexamethyldisilazide atmosphere for 10 to 20 minutes to enhance the adhesion of the silicon dioxide layer 2. The heating time must be controlled within the range of 5 to 10 minutes. If the time is too short, the photoresist 3 will flow away from the substrate in the form of water droplets during the subsequent spin coating of the photoresist 3, and the photoresist layer cannot be formed on the surface of the silicon wafer 1. If the heating time is too long, the hexamethyldisilazide film will crack.
[0075] Step a.1.2. Then, a layer of photoresist 3 is spin-coated on the outer surface of the silicon dioxide layer 2 of the mold blank treated in step a.1.1; in step a.1.2, the spin-coating parameters of the photoresist 3 are: low speed rotation speed 600~900rpm, spin-coating time 6~9s, high speed rotation speed 6000~9000rpm, spin-coating time 20~30s.
[0076] Step a.1.3. Place the mold blank processed in step a.1.2 on a hot plate for pre-baking, and then place a photolithography mask 4 on it for ultraviolet exposure with ultraviolet light 5 (such as Figure 1 The exposure time of UV exposure is 2~15s.
[0077] Step a.1.4. Place the mold blank treated in step a.1.3 on a hot plate at 100-120°C and reverse bake for 1-3 min; after cooling to room temperature, perform full exposure for 60-80 s. After developing for 40-60 s, a micron-scale inverted trapezoidal photoresist 3 step (such as Figure 1 1b). After development, a micron-scale inverted trapezoidal photoresist step is obtained. If the photolithography time is too long (>15s), the exposure amount is large and the inverted trapezoidal photoresist step cannot be formed. Specifically, the development method used in this embodiment to form a micron-scale inverted trapezoidal photoresist step is related to the properties of the photoresist 3 itself and the control of the exposure time. In this embodiment, the inverted trapezoidal photoresist step with different sidewall angles can be obtained by controlling the exposure time.
[0078] Step a.1.5. The mold blank with the micron-scale inverted trapezoidal photoresist step processed in step a.1.4 is etched with hydrofluoric acid buffer solution to etch the silicon dioxide layer 2 except the bottom of the photoresist 3 for 8 to 15 seconds (eg Figure 1 1c); then a copper film 6 is vertically deposited directly above the photoresist 3 of the mold blank, and a nano-gap is generated between the silicon dioxide layer 2 below the micron-scale inverted trapezoidal photoresist 3 step and the deposited copper film 6 (as shown in FIG. Figure 1 1d). The vertical deposition method of depositing a layer of copper film 6 vertically above the photoresist 3 of the mold blank is implemented by a thermal evaporation process in the prior art.
[0079] Step a.1.6. Soak the mold blank treated in step a.1.5 in an acetone solution for 30 to 60 minutes and then remove the photoresist 3, leaving a nano-gap (such as Figure 1 1e). The immersion time in the acetone solution must be more than 30 minutes. If the time is too short, the acetone cannot fully dissolve the photoresist 3, resulting in the difficulty of stripping and removing the photoresist 3 during the stripping process.
[0080] Step a.1.7. The mold blank processed in step a.1.6 is etched by using a reactive ion deep etching technique to etch the exposed silicon wafer 1, and a nanochannel (such as Figure 1 (as shown in 1f);
[0081] Step a.1.8. The mold blank treated in step a.1.7 is treated with hydrofluoric acid buffer to remove the remaining silicon dioxide layer 2, and the copper film 6 is removed with concentrated nitric acid to obtain a silicon nano-concave mold 7 (such as Figure 1 1g).
[0082] Step a.2. Using the silicon nano-concave mold 7 prepared in step a.1, a PDMS nano-convex mold (such as Figure 2 As shown), and there are nanoridges on the PDMS nanoconvex mold;
[0083] Further, the PDMS nanoconvex mold is manufactured by a casting method, comprising the following steps:
[0084] Step a.2.1. Place the silicon nano-concave mold 7 in dimethyldichlorosilane, toluene and ethanol solutions respectively and soak them for 15 to 30 seconds to form an anti-adhesive layer.
[0085] Step a.2.2. Pour the PDMS mixed solution 8 onto the silicon nano-concave mold 7 and place it in a vacuum environment with a vacuum degree of less than 10 Pa for at least 1 hour to allow the PDMS mixed solution 8 to completely fill the silicon nano-concave mold 7 (such as Figure 2 2a), and then placed in a 60~85℃ oven for 2~4h to solidify, and after cooling to room temperature; the PDMS nanoconvex mold formed by the solidified PDMS mixed solution 8 is separated from the silicon nanoconcave mold 7 to obtain a PDMS nanoconvex mold (as shown in Figure 2 As shown, 2b is a front view). The PDMS mixed solution 8 is in a volume ratio of 4:1 to 10:1. If the vacuum degree is greater than 10Pa or the vacuuming time is less than 1h, the PDMS mixed solution 8 cannot be completely filled into the silicon nano-concave mold 7, and the nano-ridges on the PDMS nano-convex mold are disconnected. Further, Fig. 9 As shown, it is an atomic force microscope image of the disconnection phenomenon of the nano-ridges on the PDMS nano-convex mold of the preferred embodiment of the present invention. When the vacuum degree is higher than 10Pa, the PDMS mixed solution cannot fully fill the silicon nano-concave mold, thereby causing the disconnection phenomenon of the nano-ridges on the PDMS nano-convex mold. Therefore, in the embodiment of the present invention, the vacuum degree is required to be below 10Pa.
[0086] Step a.3. Prepare the PDMS nanoconvex mold (such as Figure 3 As shown, 3c is a left view and is rotated 180°, mainly to facilitate the schematic diagram of 3D printing lines). A plurality of convex lines are 3D printed outward from one side of the nano-ridge, and a plurality of convex lines are 3D printed to form a micron channel convex mold on the PDMS nano-convex mold (such as Figure 3 3d), and a steel needle reserved connection channel convex mold connected to the micron channel convex mold; obtain a PDMS-PEO micro-nano spray needle convex mold (as shown in Figure 3 (as shown in 3e);
[0087] Furthermore, in the step of preparing the PDMS-PEO micro-nano spray needle convex mold, it also includes:
[0088] Step a.3.1. Prepare a PDMS nanoconvex mold (such as Figure 3 3c) is subjected to oxygen plasma treatment, the treatment power is 5-20W, and the treatment time is 10-30s; in order to improve the bonding force between the printing material and the PDMS nanoconvex mold, the PDMS nanoconvex mold needs to be treated with oxygen plasma before electrojet printing;
[0089] Step a.3.2. Print the micron channel convex mold (such as Figure 3 3d), and a steel needle reserved connection channel convex mold connected to the micron channel convex mold (as shown in Figure 3 3e). The 3D printing method of a plurality of convex lines includes: 3D printing a convex line with a line width of 50 mm as a micron channel convex mold, wherein the parameters are a voltage of 1500-2200 V, a concentration of 1-3 wt% PEO, and a working distance of 500-700 mm; extending the 50 mm line and then 3D printing a convex line with a line width of 100 mm as a micron channel convex mold, wherein the parameters are a voltage of 2000-2500 V, a concentration of 2-4 wt% PEO, and a working distance of 600-800 mm; and then 3D printing another convex line of 50 mm as a steel needle reserved connection channel convex mold.
[0090] Step a.4. Using the PDMS-PEO micro-nano spray needle convex mold prepared in step a.3, an unbonded polymer micro-nano spray needle (such as Figure 3 As shown in 3f, the unbonded polymer micro-nano spray needle has a reserved micron channel and a reserved connection channel of a steel needle connected to the micron channel (as shown in Figure 3 3g). The depth of the micron channel is greater than the depth of the nano channel, and the combination forms a step-by-step gradually narrowing path extending from the micron channel to the tip of the unbonded polymer micro-nano spray needle nano needle.
[0091] The method of using a casting method to cast a PDMS-PEO micro-nano spray needle convex mold to obtain an unbonded polymer micro-nano spray needle comprises:
[0092] Step a.4.1. Place the PDMS-PEO micro-nano spray needle convex mold in a drying tower filled with trimethylchlorosilane atmosphere and let it stand for 5 to 20 minutes;
[0093] Step a.4.2. Pour the mixed PDMS mixed solution 8 into the PDMS-PEO micro-nano spray needle convex mold, and place it in a vacuum environment below 10Pa and evacuate for 1~2h to ensure that PDMS completely fills the PDMS-PEO micro-nano spray needle convex mold; the volume ratio of the PDMS mixed solution 8 is 4:1~10:1.
[0094] Step a.4.3. Place in an oven at 60-85°C and bake for 2-4 hours to solidify. After cooling to room temperature, separate the unbonded polymer micro-nano spray needle formed after the PDMS mixed solution 8 is solidified from the PDMS-PEO micro-nano spray needle convex mold to obtain an unbonded polymer micro-nano spray needle.
[0095] Specifically, the preparation method of the PDMS needle cover plate includes:
[0096] Step b.1. Obtain a glass substrate, perform a hydrophilic treatment on the glass substrate, and print a convex line on the hydrophilic treated glass substrate. In this embodiment, the convex line in step b.1 is a short line with a width of 50 mm, and a convex mold of a nozzle cover plate is obtained; the convex mold of the nozzle cover plate is then placed in a trimethylchlorosilane atmosphere for hydrophobic treatment, and the treatment time is 5 to 20 minutes. More preferably, the printing voltage is controlled at 1500 to 2100 V, and the PEO concentration is 1 to 3 wt%; in other embodiments, the electrojet printing ink PEO can be replaced with PVP, and its PVP concentration is 1 to 5 wt%. Step b.2. Pour the PDMS mixed solution on the nozzle cover plate convex mold, and place it in a 60 to 85 ° C oven for 2 to 4 hours to cure. The volume ratio of the PDMS mixed solution is 4:1 to 10:1 PDMS and curing agent. Then cool to room temperature and separate from the nozzle cover plate convex mold to obtain a PDMS nozzle cover plate with a reserved channel for a steel needle.
[0097] In a preferred embodiment of the present invention, the photoresist 3 adopts AZ701, AZ703, AZ5214E, AR-N4240, AR-N4340, AR-P5300, AR-N4400, AR-U4000, BP212, BN308, NR26-8000P, PR1-1500A1, or SU-8 photoresist; in this embodiment, the photoresist 3 adopts AZ5214E photoresist.
[0098] In a preferred embodiment of the present invention, the copper film 6 can be replaced by Al, Cr, Au, Ag, SiO2 or Ni; and the nitric acid can be replaced by aqua regia. Embodiment 2
[0099] On the basis of the first embodiment, after step S3, step S4 is further included, wherein the polymer micro-nano spray needle processed in step S3 is subjected to shape trimming, and the shape trimming includes cutting off excess PDMS material to obtain the spray needle contour, thereby obtaining a plug-and-play micro-nano spray needle (such as Figure 5 as shown). Embodiment 3
[0100] A micro-nano spray needle is prepared by using a plug-and-play micro-nano spray needle manufacturing method of embodiment 1 or embodiment 2 (such as Figure 6as shown).
[0101] Working principle:
[0102] The spray needle prepared by the present invention is equipped with a steel pipe suitable for direct connection with the ink supply system, which can achieve a plug-and-play effect. Since the spray needle is very easy to get clogged during the printing process and belongs to a printing consumable, plug-and-play greatly improves the printing efficiency and convenience of use.
[0103] The above specific implementation methods are specific support for the scheme ideas proposed in the present invention, and cannot be used to limit the protection scope of the present invention. Any equivalent changes or equivalent modifications made on the basis of this technical scheme in accordance with the technical ideas proposed in the present invention still fall within the scope of protection of the technical scheme of the present invention.
Claims
1. A plug-and-play micro-nano spray needle manufacturing method, characterized in that: The following steps are involved: Step S1. treating the PDMS needle cover plate and the unbonded polymer micro-nano needle with oxygen plasma; The preparation method of the unbonded polymer micro-nano spray needle comprises: Step a.
1. Prepare a silicon nanoconcave mold by using an angle molding peeling method; Step a.
2. Using the silicon nano-concave mold prepared in step a.1, a PDMS nano-convex mold is obtained by casting, and the PDMS nano-convex mold has nano-ridges; Step a.
3. Print a plurality of convex lines extending outward from one side of the nano-ridge of the PDMS nano-convex mold prepared in step a.2, print a plurality of convex lines to form a micron channel convex mold on the PDMS nano-convex mold, and a steel needle reserved connection channel convex mold connected to the micron channel; obtain a PDMS-PEO micro-nano spray needle convex mold; Step a.
4. The PDMS-PEO micro-nano spray needle convex mold prepared in step a.3 is used to obtain an unbonded polymer micro-nano spray needle by a casting method, wherein the unbonded polymer micro-nano spray needle is provided with a reserved connection channel for a microchannel steel needle; the depth of the micron channel is greater than the depth of the nano channel, and the micron channel is combined to form a step-by-step gradually narrowing passage extending from the micron channel to the nano needle tip of the polymer micro-nano spray needle; The preparation method of the PDMS needle cover plate comprises: Step b.
1. Obtain a glass substrate, perform a hydrophilic treatment on the glass substrate, and print a convex line on the hydrophilic treated glass substrate; the convex line in step b.1 is a 50 mm convex line; Step b.
2. Pour the PDMS mixed solution onto the glass substrate, and place it in an oven at 60-85°C for 2-4 hours for curing. After cooling to room temperature, separate it from the glass substrate to obtain a PDMS needle cover with a reserved channel for the steel needle. Step S2. Then aligning and bonding the PDMS needle cover plate with the reserved channel of the steel needle with the unbonded polymer micro-nano needle to seal the micro-nano channel of the needle and obtain the polymer micro-nano needle; Step S3. inserting the hydrophilic treated steel needle into the reserved connection channel of the polymer micro-nano spray needle for interference fit; The angle forming peeling method is used to prepare a silicon nano-concave mold, which includes the following steps: Step a.1.
1. Place the silicon wafer with the silicon dioxide layer as a mold blank in a drying tower filled with hexamethyldisilazane atmosphere for 10 to 20 minutes to enhance the adhesion between the silicon dioxide layer and the photoresist; Step a.1.
2. Then, a layer of photoresist is spin-coated on the outer surface of the silicon dioxide layer of the mold blank treated in step a.1.1; in step a.1.2, the spin coating parameters of the photoresist are: low speed 600~900rpm, spin coating time 6~9s, high speed 6000~9000rpm, spin coating time 20~30s; Step a.1.
3. Place the mold blank processed in step a.1.2 on a hot plate for pre-baking and then UV exposure; Step a.1.
4. Place the mold blank treated in step a.1.3 on a hot plate at 100-120°C and reverse bake for 1-3 minutes; after cooling to room temperature, perform full exposure for 60-80 seconds, and after developing for 40-60 seconds, form a micron-scale inverted trapezoidal photoresist step on the mold blank; Step a.1.
5. The mold blank with the micron-scale inverted trapezoidal photoresist step processed in step a.1.4 is etched with a hydrofluoric acid buffer solution for 8 to 15 seconds to etch away the silicon dioxide layer except for the bottom of the photoresist; then a layer of copper film is vertically deposited directly above the photoresist of the mold blank, and a nano-gap is generated between the silicon dioxide layer below the micron-scale inverted trapezoidal photoresist step and the deposited copper film; Step a.1.
6. Soak the mold blank treated in step a.1.5 in an acetone solution for 30 to 60 minutes, then peel off and remove the photoresist, leaving a nano-gap between the silicon dioxide layer on the mold blank and the deposited copper film; Step a.1.
7. The mold blank processed in step a.1.6 is etched using a reactive ion deep etching technique to etch the exposed silicon wafer, thereby forming a nanochannel on the silicon wafer; Step a.1.
8. Using hydrofluoric acid buffer to remove the remaining silicon dioxide layer from the mold blank treated in step a.1.7, and using concentrated nitric acid to remove the copper film, to obtain a silicon nano-concave mold; The PDMS nanoconvex mold is manufactured by a casting method, comprising the following steps: Step a.2.
1. Place the silicon nanoconcave mold in dimethyldichlorosilane, toluene and ethanol solutions respectively and soak for 15 to 30 seconds to form an anti-adhesive layer; Step a.2.
2. Pour the PDMS mixed solution onto the silicon nano-concave mold, place it in a vacuum environment with a vacuum degree of less than 10Pa for at least 1 hour, so that the PDMS mixed solution completely fills the silicon nano-concave mold, and then place it in a 60-85°C oven for 2-4 hours to cure, and cool to room temperature; separate the PDMS nano-convex mold formed by the cured PDMS mixed solution from the silicon nano-concave mold to obtain a PDMS nano-convex mold; The step of preparing the PDMS-PEO micro-nano spray needle convex mold also includes: Step a.3.
1. The PDMS nanoconvex mold is treated with oxygen plasma at a treatment power of 5 to 20 W and a treatment time of 10 to 30 seconds. In order to improve the bonding force between the printing material and the PDMS nanoconvex mold, the PDMS nanoconvex mold is treated with oxygen plasma before electrojet printing. Step a.3.
2. Printing the micron channel convex mold and the steel needle reserved connection channel convex mold on the PDMS nanoconvex mold after oxygen plasma treatment; In step a.3.2, the method for printing a plurality of convex lines includes: Print a 50mm wide convex line with the parameters of voltage 1500~2200V, concentration 1~3wt% PEO, and working distance 500~700mm as a microchannel convex mold; extend the 50mm line and then print a 100mm wide convex line with the parameters of voltage 2000~2500V, concentration 2~4wt% PEO, and working distance 600~800mm as a microchannel convex mold; then extend the 100mm line and print another 50mm convex line as a steel needle reserved connection channel convex mold.
2. The plug-and-play micro-nano spray needle manufacturing method according to claim 1, characterized in that: In step S1, the processing power of the oxygen plasma treatment is 5-20W, and the processing time is 10-30s; and\or, in step b.2, the volume ratio of the PDMS mixed solution is 4:1 to 10:1 of PDMS and curing agent; and\or, in step S3, one end of the steel needle is inserted into the steel needle reserved connection channel of the polymer micro-nano spray needle and communicated with the microchannel, and the other end of the steel needle is located outside the polymer micro-nano spray needle; And\or, in step a.1.3, the pre-baking is to place the silicon wafer spin-coated with the photoresist on a 100-120°C hot plate for pre-baking for 1-3 minutes; the exposure time of the ultraviolet exposure is 2-15 seconds; In step a.2.2, the volume ratio of the PDMS mixed solution is 4:1~10:
1.
3. The plug-and-play micro-nano spray needle manufacturing method according to claim 2, characterized in that: The method of using a casting method to cast a PDMS-PEO micro-nano spray needle convex mold to obtain an unbonded polymer micro-nano spray needle comprises: Step a.4.
1. Place the PDMS-PEO micro-nano spray needle convex mold in a drying tower filled with trimethylchlorosilane atmosphere and let it stand for 5 to 20 minutes; Step a.4.
2. Pour the mixed PDMS solution onto the PDMS-PEO micro-nano spray needle convex mold, and place it in a vacuum oven to evacuate for 1-2 hours to ensure that the PDMS mixed solution completely fills the PDMS-PEO micro-nano spray needle convex mold; Step a.4.
3. Place the PDMS-PEO micro-nano spray needle convex mold cast with the PDMS mixed solution in a 60~85℃ oven and bake for 2~4 hours to solidify. After cooling to room temperature, separate the unbonded polymer micro-nano spray needle formed after the PDMS mixed solution is solidified from the mold to obtain an unbonded polymer micro-nano spray needle.
4. The plug-and-play micro-nano spray needle manufacturing method according to claim 3, characterized in that: The photoresist used is AZ701, AZ703, AZ5214E, AR-N4240, AR-N4340, AR-P5300, AR-N4400, AR-U4000, BP212, BN308, PR1-1500A1, or SU-8 photoresist; And / or, the copper film can be replaced by Al, Cr, Au, Ag, SiO2 or Ni; and the nitric acid can be replaced by aqua regia.
5. The plug-and-play micro-nano spray needle manufacturing method according to claim 4, characterized in that: In step b.2, the volume ratio of the PDMS mixed solution is 4:1~10:1; the curing temperature is 60°~85°C, and the curing time is 2~4h; And / or, in step b.1, convex lines are printed, the printing voltage is controlled at 1500~2100V, the material used is PEO printing material or PVP printing material, the PEO concentration of PEO printing material is 1~3wt%; the PVP concentration of PVP printing material is 1~5wt%; the convex lines printed in step b.1 are subjected to atmosphere treatment with trimethylchlorosilane for 5~20min.
6. The plug-and-play micro-nano spray needle manufacturing method according to claim 5, characterized in that: After step S3, step S4 is also included, in which the polymer micro-nano spray needle processed in step S3 is subjected to shape trimming. The shape trimming includes cutting off excess PDMS material to obtain the spray needle contour, thereby obtaining a plug-and-play micro-nano spray needle.
7. A micro-nano spray needle, characterized in that: The plug-and-play micro-nano spray needle is prepared by the manufacturing method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Manufacturing method of micro-nano trans-scale polymer spray needle
CN111977611A
Method for manufacturing polymer spray needle below 100nm based on near-field electrospinning