A kind of high carbon chromium bearing steel and heat treatment method thereof
Through the heat treatment method of twice salt quenching, a bainite-martensite complex phase structure is generated, which solves the problem of uneven carbide distribution in the heat treatment of traditional high-carbon chromium bearing steel, improves the strength and toughness of bearing steel, and meets the requirements of Performance requirements of bearing steel in service environment.
Patent Information
- Application Number
- CN202410692270.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-31
AI Technical Summary
In the heat treatment process of traditional high-carbon chromium bearing steel, there are coarse and unevenly distributed carbides, which makes the bearing steel prone to cracking, poor toughness, and poor load-bearing capacity, making it difficult to effectively improve its strength and toughness.
The heat treatment method of twice salt quenching is used to generate a specific proportion of bainite-martensite complex structure through isothermal spheroidizing annealing and rapid austenitization, omitting the tempering step and shortening the heat treatment time.
While sacrificing a small amount of hardness, the strength and toughness of high-carbon chromium bearing steel are greatly improved, and a uniformly distributed bainite-martensite complex structure is formed, which significantly improves the overall performance and is suitable for various bearing steels. Market application.
Smart Images

Figure CN118441127B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high carbon chromium bearing steel, and in particular to a high carbon chromium bearing steel and a heat treatment method thereof. Background Art
[0002] Bearing steel is steel used to make balls, rollers and bearing rings. Bearing steel requires high and uniform hardness and wear resistance, as well as a high elastic limit. Therefore, the uniformity of the chemical composition of bearing steel, the content and distribution of non-metallic inclusions, the distribution of carbides, etc. are very strict. It is one of the most stringent steel grades in all steel production. High carbon chromium bearing steel GCr15 is the world's most produced bearing steel, with a carbon content of about 1% Wc and a chromium content of about 1.5% Wcr. With the advancement of science and technology, its product quality has been continuously improved, accounting for more than 80% of the world's total bearing steel production. It is often used to manufacture various bearing rings with a wall thickness of ≤12mm and an outer diameter of ≤250mm, and is also used for rolling elements with a wide range of sizes.
[0003] According to the various service environments of high carbon chromium bearing steel, after high carbon chromium bearing steel is rolled out, it is often necessary to perform a heat treatment process to ensure that it has certain properties. Spheroidizing annealing can ensure that high carbon chromium bearing steel has good machinability, and quenching and tempering can ensure that high carbon chromium bearing steel has high and uniform hardness, high wear resistance and contact fatigue resistance. However, in the traditional heat treatment process, there are coarse and unevenly distributed carbides in the structure of high carbon chromium bearing steel, and the martensite formed in the subsequent quenching and tempering process has a single performance, which makes the resulting bearing steel easy to crack, poor toughness, and poor load bearing capacity. Therefore, there is an urgent need to find a heat treatment method that can more effectively improve the comprehensive properties of high carbon chromium bearing steel such as strength and toughness. Summary of the invention
[0004] In view of the above problems, the present invention provides a high carbon chromium bearing steel and a heat treatment method thereof. Through two salt quenchings, not only a specific proportion of bainite-martensite multiphase structure is obtained, which greatly improves the strength and toughness of the high carbon chromium bearing steel at the expense of a small part of the hardness, but also omits the tempering step, saving the time cost of heat treatment.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0007] S1, subjecting the rolled bearing steel blank to isothermal spheroidizing annealing treatment to obtain bearing steel containing spheroidal carbide structure;
[0008] S2, heating the bearing steel containing spheroidal carbide structure to A at a rate of 350-450°C / min c1 ~A ccm temperature, isothermal austenitizing; then the first salt quenching is carried out at 220~240℃; the second salt quenching is carried out at 150~160℃, and cooled to room temperature to obtain high carbon chromium bearing steel.
[0009] It should be noted that A c1 is the temperature at which lamellar pearlite begins to form austenite, A ccm It is the temperature at which cementite and carbides are completely integrated into austenite.
[0010] Compared with the prior art, the heat treatment method of high carbon chromium bearing steel provided by the present invention first performs isothermal spheroidizing annealing treatment on the rolled bearing steel blank to obtain a uniformly dispersed spheroidal carbide structure to prepare the structure for quenching treatment; rapid heating can shorten the overall time of isothermal austenitization, increase the diffusion rate of elements, and cooperate with isothermal austenitization to make C and Cr elements quickly reach a uniform distribution state in austenite and spheroidal carbides, thereby accelerating the dissolution of spheroidal carbides and optimizing the morphology and distribution of undissolved spheroidal carbides; through the first salt quenching at a specific temperature, While avoiding the formation of pearlite, a part of lower bainite is generated in the bainite isothermal range, ensuring that the bearing steel has a certain toughness; through the second salt quenching at a specific temperature, while martensite is generated in the martensite isothermal range, another part of lower bainite is also generated through a certain period of heat preservation, ensuring that the bearing steel has a certain hardness and toughness, and significantly shortening the heat treatment time; and a certain period of martensite isothermal (second salt quenching) will also temper the martensite structure, thereby eliminating the tempering step after quenching treatment and shortening the overall heat treatment time to a greater extent. The present invention can ensure that the high-carbon chromium bearing steel forms a uniformly distributed bainite-martensite complex phase structure through two salt quenchings (first salt quenching and second salt quenching) at a specific temperature, thereby achieving a better combination of strength and toughness, so that the comprehensive performance of the high-carbon chromium bearing steel is optimized, and can better meet the performance required by the bearing steel in the service environment, and has a high market application value.
[0011] For example, the high carbon chromium bearing steel may be GCr15, GCr15SiMn, ZGCr15 or ZGCr15SiMn.
[0012] Preferably, in step S1, the isothermal spheroidizing annealing treatment comprises:
[0013] The bearing steel blank is placed in a heat treatment furnace, heated to 780-820°C at a rate of 8-12°C / min, and kept warm for 30-40min; then cooled to 700-720°C with the furnace, and kept warm for 60-90min; then cooled to 640-660°C with the furnace, and air-cooled to room temperature after being taken out of the furnace.
[0014] In step S1 of the present invention, the bearing steel blank is subjected to a first isothermal transformation at 780-820°C, so that its structure is partially austenitized, the lamellar pearlite is melted and gradually formed into a spherical shape, and a large amount of undissolved spherical carbides are retained; then a second isothermal transformation is carried out at 700-720°C, and its ferrite and cementite grow in a non-synergistic manner. As the isothermal time is extended, the interface between ferrite and austenite continues to advance, and the excess carbide-forming elements in the austenite will directly accumulate, nucleate and grow on the existing undissolved spherical carbides, and finally the austenite is transformed into a spherical carbide structure; then in the subsequent cooling process, the lamellar cementite in the pearlite gradually becomes spherical, so that the bearing steel obtains a large amount of spherical carbide structure while refining the carbides, and prepares the structure for quenching treatment.
[0015] Preferably, in step S2, electric pulses are used for heating to achieve a heating rate of 350-450°C / min.
[0016] Further preferably, in step S2, the pulse frequency of the electric pulse is 600-1000 Hz, and the current density is 30-50 A / mm 2 .
[0017] Preferably, in step S2, the isothermal austenitizing temperature is 840-860° C., and the holding time is 5-10 min.
[0018] Preferably, in step S2, the holding time of the first salt quenching is 10 to 30 minutes.
[0019] Preferably, in step S2, the holding time of the second salt quenching is 20 to 30 minutes.
[0020] Preferably, in step S2, oil cooling is used to cool to room temperature.
[0021] The present invention limits the conditions of step S2 (i.e., bainite-martensite dual-phase quenching treatment) to make isothermal austenitization more uniform and sufficient, thus preparing for the subsequent transformation of bainite-martensite dual-phase structure; 15%-20% of lower bainite can be generated during the first salt quenching (bainite isothermal) process, and 40%-45% of martensite and 10%-15% of lower bainite can be generated during the second salt quenching (martensite isothermal) process, which can greatly improve the toughness of high carbon chromium bearing steel while slightly reducing the hardness, ensure that the bearing steel has optimal toughness and strength, and greatly improve the overall performance.
[0022] In a second aspect, the present invention provides a high carbon chromium bearing steel prepared by the above-mentioned heat treatment method for high carbon chromium bearing steel.
[0023] Preferably, the high carbon chromium bearing steel consists of the following chemical components in terms of mass percentage: C 0.95%~1.05%, Si 0.15%~0.35%, Mn 0.25%~0.45%, Cr 1.40%~1.65%, Mo≤0.10%, P≤0.025%, S≤0.025%, Ni≤0.30%, Cu≤0.25%, and the remainder is Fe; wherein, Ni+Cu≤0.50%.
[0024] Preferably, in the high carbon chromium bearing steel, the lower bainite content is 28% to 35%, and the martensite content is 40% to 45%.
[0025] The high carbon chromium bearing steel provided by the present invention contains a uniformly distributed bainite-martensite multiphase structure. The results of the embodiment show that its tensile strength can reach more than 2700MPa and its impact toughness can reach 9.5kJ / mm 2 The above is suitable for large-scale production and has good market application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic flow chart of a heat treatment method for high carbon chromium bearing steel provided by the present invention;
[0027] Figure 2 A scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Example 1 of the present invention;
[0028] Figure 3 A scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Example 2 of the present invention;
[0029] Figure 4 A scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Example 3 of the present invention;
[0030] Figure 5 This is a scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Comparative Example 1 of the present invention;
[0031] Figure 6 This is a scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Comparative Example 2 of the present invention;
[0032] Figure 7 This is a scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Comparative Example 3 of the present invention;
[0033] Figure 8 This is a scanning electron microscope image of the microstructure of the high carbon chromium bearing steel provided in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0035] See also Figure 1 The present invention provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0036] S1, placing the rolled bearing steel blank into a heat treatment furnace for isothermal spheroidizing annealing treatment: performing the first isothermal transformation at 780-820°C and the second isothermal transformation at 700-720°C; then cooling the blank to 640-660°C with the furnace, and air cooling the blank to room temperature to obtain a bearing steel containing spheroidal carbide structure;
[0037] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite dual phase quenching treatment: firstly heating the bearing steel to A at a rate of 350-450°C / min; c1 ~A ccm temperature, isothermal austenitization; then the first salt quenching is carried out at 220-240°C; the second salt quenching is carried out at 150-160°C, and oil cooling is carried out to room temperature to obtain high carbon chromium bearing steel;
[0038] Among them, A c1 is the temperature at which lamellar pearlite begins to form austenite, A ccm It is the temperature at which cementite and carbides are completely integrated into austenite.
[0039] The heat treatment method of high carbon chromium bearing steel provided by the present invention is applicable to GCr15 and related steel grades. In order to better illustrate the present invention, the high carbon chromium bearing steel used in the embodiments and comparative examples of the present invention is GCr15.
[0040] In order to better illustrate the present invention, further examples are given below.
[0041] Example 1
[0042] This embodiment provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0043] S1, the rolled bearing steel blank is placed in a heat treatment furnace for isothermal spheroidizing annealing treatment: the temperature is raised to 780°C at a rate of 8°C / min, the first isothermal transformation is carried out, and the temperature is kept for 40 minutes; then the blank is cooled to 700°C with the furnace, the second isothermal transformation is carried out, and the temperature is kept for 88 minutes; then the blank is cooled to 640°C with the furnace, and the blank is air-cooled to room temperature after being taken out of the furnace to obtain a bearing steel containing spheroidal carbide structure.
[0044] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite dual phase quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 600 Hz, the current density is 40 A / mm 2 ), the temperature was raised to 840°C at a rate of 350°C / min, isothermally austenitized, and kept warm for 10 minutes; the austenitized bearing steel was placed in a salt bath furnace at 220°C without stagnation, subjected to the first salt quenching, and kept warm for 30 minutes; then placed in a salt bath furnace at 160°C, subjected to the second salt quenching, and kept warm for 20 minutes, and oil-cooled to room temperature to obtain high carbon chromium bearing steel.
[0045] Calculated in percentage by mass, the high carbon chromium bearing steel consists of the following chemical components: C 0.95%, Si 0.15%, Mn 0.45%, Cr 1.65%, Mo 0.05%, P 0.01%, S 0.02%, Ni 0.25%, Cu 0.15%, and the remainder is Fe.
[0046] The high carbon chromium bearing steel prepared in this example was scanned by electron microscope, and the microstructure observed was as follows: Figure 2 As shown in the figure, it can be seen that the high carbon chromium bearing steel prepared in this embodiment is composed of martensite, lower bainite, spheroidal carbide and residual austenite. According to the test, the high carbon chromium bearing steel prepared in this embodiment contains 30% lower bainite and 45% martensite.
[0047] Example 2
[0048] This embodiment provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0049] S1, the rolled bearing steel blank is placed in a heat treatment furnace for isothermal spheroidizing annealing treatment: the temperature is raised to 800°C at a rate of 10°C / min, the first isothermal transformation is carried out, and the temperature is kept for 35 minutes; then the blank is cooled to 720°C with the furnace, the second isothermal transformation is carried out, and the temperature is kept for 62 minutes; then the blank is cooled to 650°C with the furnace, and the blank is air-cooled to room temperature after being taken out of the furnace to obtain a bearing steel containing spheroidal carbide structure.
[0050] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite dual phase quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 800 Hz, the current density is 30 A / mm 2 ), the temperature was raised to 850°C at a rate of 390°C / min, isothermally austenitized, and kept warm for 8 minutes; the austenitized bearing steel was placed in a salt bath furnace at 230°C without stagnation, subjected to the first salt quenching, and kept warm for 20 minutes; then placed in a salt bath furnace at 150°C, subjected to the second salt quenching, and kept warm for 30 minutes, and oil-cooled to room temperature to obtain high carbon chromium bearing steel.
[0051] Calculated in percentage by mass, the high carbon chromium bearing steel consists of the following chemical components: C 1%, Si 0.2%, Mn 0.28%, Cr 1.5%, Mo 0.05%, P 0.01%, S 0.02%, Ni 0.25%, Cu 0.1%, and the remainder is Fe.
[0052] The high carbon chromium bearing steel prepared in this example was scanned by electron microscope, and the microstructure observed was as follows: Figure 3 As shown in the figure, it can be seen that the high carbon chromium bearing steel prepared in this embodiment is composed of martensite, lower bainite, spheroidal carbide and residual austenite. After testing, the high carbon chromium bearing steel prepared in this embodiment contains 34% lower bainite and 44% martensite.
[0053] Example 3
[0054] This embodiment provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0055] S1, the rolled bearing steel blank is placed in a heat treatment furnace for isothermal spheroidizing annealing treatment: the temperature is raised to 820°C at a rate of 12°C / min, the first isothermal transformation is carried out, and the temperature is kept for 35 minutes; then the blank is cooled to 710°C with the furnace, the second isothermal transformation is carried out, and the temperature is kept for 75 minutes; then the blank is cooled to 660°C with the furnace, and the blank is air-cooled to room temperature after being taken out of the furnace to obtain a bearing steel containing spheroidal carbide structure.
[0056] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite dual phase quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 1000 Hz, the current density is 45 A / mm 2 ), the temperature was raised to 860°C at a rate of 420°C / min, isothermally austenitized, and kept warm for 5 minutes; the austenitized bearing steel was placed in a salt bath furnace at 240°C without stagnation, subjected to the first salt quenching, and kept warm for 10 minutes; then placed in a salt bath furnace at 160°C, subjected to the second salt quenching, and kept warm for 20 minutes, and oil-cooled to room temperature to obtain high carbon chromium bearing steel.
[0057] Calculated in percentage by mass, the high carbon chromium bearing steel consists of the following chemical components: C 1.05%, Si 0.35%, Mn 0.25%, Cr 1.4%, Mo 0.05%, P 0.01%, S 0.02%, Ni 0.2%, Cu 0.2%, and the remainder is Fe.
[0058] The high carbon chromium bearing steel prepared in this example was scanned by electron microscope, and the microstructure observed was as follows: Figure 4 As shown in the figure, it can be seen that the high carbon chromium bearing steel prepared in this embodiment is composed of martensite, lower bainite, spheroidal carbide and residual austenite. After testing, the high carbon chromium bearing steel prepared in this embodiment contains 35% lower bainite and 40% martensite.
[0059] Example 4
[0060] This embodiment provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0061] S1, the rolled bearing steel blank is placed in a heat treatment furnace for isothermal spheroidizing annealing treatment: the temperature is raised to 790°C at a rate of 11°C / min, the first isothermal transformation is carried out, and the temperature is kept for 37 minutes; then the blank is cooled to 710°C with the furnace, the second isothermal transformation is carried out, and the temperature is kept for 80 minutes; then the blank is cooled to 650°C with the furnace, and the blank is air-cooled to room temperature after being taken out of the furnace to obtain a bearing steel containing spheroidal carbide structure.
[0062] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite dual phase quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 900 Hz, the current density is 50 A / mm 2 ), the temperature was raised to 850°C at a rate of 440°C / min, isothermally austenitized, and kept warm for 7 minutes; the austenitized bearing steel was placed in a salt bath furnace at 230°C without stagnation, subjected to the first salt quenching, and kept warm for 20 minutes; then placed in a salt bath furnace at 155°C, subjected to the second salt quenching, and kept warm for 25 minutes, and oil-cooled to room temperature to obtain high carbon chromium bearing steel.
[0063] Calculated in percentage by mass, the high carbon chromium bearing steel consists of the following chemical components: C 1%, Si 0.25%, Mn 0.3%, Cr 1.55%, Mo 0.05%, P 0.01%, S 0.02%, Ni 0.25%, Cu 0.15%, and the remainder is Fe.
[0064] According to tests, the high carbon chromium bearing steel prepared in this embodiment contains 32% lower bainite and 42% martensite.
[0065] Comparative Example 1
[0066] This comparative example provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0067] S1 is the same as Example 2 (the chemical composition of the bearing steel blank is also the same as that of Example 2), and will not be repeated here.
[0068] S2, subjecting the bearing steel containing the spheroidal carbide structure to a martensitic quenching treatment: firstly heating the temperature to 850°C at a rate of 10°C / min, performing isothermal austenitization, keeping the temperature for 30 minutes, and then directly oil cooling to room temperature to obtain a bearing steel with a martensitic structure.
[0069] S3, tempering the bearing steel having a martensitic structure at 160° C. for 3 hours to obtain high carbon chromium bearing steel.
[0070] The high carbon chromium bearing steel prepared in this comparative example was subjected to electron microscope scanning, and the microstructure observed was as follows: Figure 5 As shown in the figure, it can be seen that the high carbon chromium bearing steel prepared in this comparative example is a completely martensitic structure (composed of martensite, spherical carbides and retained austenite).
[0071] Comparative Example 2
[0072] This comparative example provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0073] S1 is the same as Example 2 (the chemical composition of the bearing steel blank is also the same as that of Example 2), and will not be repeated here.
[0074] S2, subjecting the above-mentioned bearing steel containing spheroidal carbide structure to bainite quenching treatment: firstly heating to 850°C at a rate of 10°C / min, isothermally austenitizing, and keeping warm for 30 minutes; continuously placing the obtained austenitized bearing steel into a salt bath furnace at 230°C, salt quenching, and keeping warm for 4 hours; and oil cooling to room temperature to obtain bearing steel with lower bainite structure.
[0075] S3, tempering the bearing steel with lower bainite structure at 160° C. for 3 hours to obtain high carbon chromium bearing steel.
[0076] The high carbon chromium bearing steel prepared in this comparative example was subjected to electron microscope scanning, and the microstructure observed was as follows: Figure 6 As shown in the figure, it can be seen that the high carbon chromium bearing steel prepared in this comparative example is a complete lower bainite structure (composed of lower bainite, spherical carbides and retained austenite).
[0077] Comparative Example 3
[0078] This comparative example provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0079] S1 is the same as Example 2 (the chemical composition of the bearing steel blank is also the same as that of Example 2), and will not be repeated here.
[0080] S2, subjecting the bearing steel containing spheroidal carbide structure to martensite-bainite quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 800 Hz, the current density is 30 A / mm 2 ), the temperature was raised to 850°C at a rate of 390°C / min, isothermally austenitized, and kept warm for 8 minutes; the austenitized bearing steel was placed in a salt bath furnace at 150°C without stagnation for the third salt quenching (martensite isothermal), and kept warm for 1 minute; then placed in a salt bath furnace at 230°C for the fourth salt quenching (bainite isothermal), and kept warm for 240 minutes, and oil-cooled to room temperature to obtain a bearing steel with a martensite-bainite duplex structure.
[0081] S3, tempering the bearing steel having the martensite-bainite dual phase structure at 160° C. for 3 h (to eliminate stress) to obtain high carbon chromium bearing steel.
[0082] The high carbon chromium bearing steel prepared in this comparative example was subjected to electron microscope scanning, and the microstructure observed was as follows: Figure 7 As shown. After testing, the high carbon chromium bearing steel prepared in this comparative example contains 35% lower bainite and 39% martensite; it can be seen from the figure that the high carbon chromium bearing steel is composed of tempered martensite, lower bainite, spheroidal carbide and residual austenite, but its martensite is lath-shaped and coarse, and the coarse martensite is very easy to crack during use, thereby greatly reducing the toughness of the high carbon chromium bearing steel.
[0083] Comparative Example 4
[0084] This comparative example provides a heat treatment method for high carbon chromium bearing steel, comprising the following steps:
[0085] S1 is the same as Example 2 (the chemical composition of the bearing steel blank is also the same as that of Example 2), and will not be repeated here.
[0086] S2, subjecting the bearing steel containing spheroidal carbide structure to bainite-martensite quenching treatment: heating by passing electric pulse (the pulse frequency of the electric pulse is 800 Hz, the current density is 30 A / mm 2 ), the temperature was raised to 850°C at a rate of 390°C / min for isothermal austenitization, and the temperature was kept at this temperature for 8 minutes; the austenitized bearing steel was continuously placed in a salt bath furnace at 230°C for the first salt quenching, and the temperature was kept at this temperature for 30 minutes, and the bearing steel was oil-cooled to room temperature to obtain a bearing steel with a martensite-bainite duplex structure.
[0087] S3, tempering the bearing steel having the martensite-bainite dual phase structure at 160° C. for 3 h (to eliminate stress) to obtain high carbon chromium bearing steel.
[0088] The high carbon chromium bearing steel prepared in this comparative example was subjected to electron microscope scanning, and the microstructure observed was as follows: Figure 8 As shown. After testing, the high carbon chromium bearing steel prepared in this comparative example contains 33% lower bainite and 40% martensite; it can be seen from the figure that the high carbon chromium bearing steel is composed of martensite, lower bainite, spheroidal carbide and residual austenite, but after the quenching process, a long low temperature tempering process is required to eliminate the stress caused by the martensitic structure and improve a certain toughness.
[0089] Performance Testing
[0090] The high carbon chromium bearing steels of Examples 1 to 4 and Comparative Examples 1 to 4 were respectively subjected to mechanical property tests, and the test results are shown in Table 1. It can be seen from Table 1 that the high carbon chromium bearing steels provided in Examples 1 to 4 of the present invention can achieve a better combination of strength and toughness (higher strength, toughness and wear resistance) at the expense of a small hardness; the high carbon chromium bearing steel provided in Comparative Example 1 has high hardness, but poor toughness, and the overall heat treatment time is long; the high carbon chromium bearing steel provided in Comparative Example 2 has a toughness that meets the standard, but poor hardness and strength, and the overall heat treatment time is long; the high carbon chromium bearing steels provided in Comparative Examples 3 and 4, although under the action of the bainite-martensite complex phase structure, ensure the hardness and toughness of the steel, but require a long low-temperature tempering process, and at the same time, the time for other heat treatments in Comparative Example 3 except tempering is also longer than the heat treatment time of the embodiments of the present invention, which prolongs the overall heat treatment time.
[0091] Table 1 Mechanical properties test results of high carbon chromium bearing steel of examples and comparative examples
[0092]
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A heat treatment method for high carbon chromium bearing steel, characterized in that: It includes the following steps: S1, subjecting the rolled bearing steel blank to isothermal spheroidizing annealing treatment to obtain bearing steel containing spheroidal carbide structure; S2, heating the bearing steel containing spheroidal carbide structure to A at a rate of 350-450°C / min c1 ~A ccm temperature, isothermal austenitizing; then a first salt quenching is performed at 220-240°C; a second salt quenching is performed at 150-160°C, and the steel is cooled to room temperature by oil cooling to obtain high carbon chromium bearing steel; in the high carbon chromium bearing steel, the lower bainite content is 28%-35%, and the martensite content is 40%-45%.
2. The heat treatment method of high carbon chromium bearing steel according to claim 1, characterized in that: In step S1, the isothermal spheroidizing annealing treatment includes: The bearing steel blank is placed in a heat treatment furnace, heated to 780-820°C at a rate of 8-12°C / min, and kept warm for 30-40min; then cooled to 700-720°C with the furnace, and kept warm for 60-90min; then cooled to 640-660°C with the furnace, and air-cooled to room temperature after being taken out of the furnace.
3. The heat treatment method of high carbon chromium bearing steel according to claim 1 or 2, characterized in that: In step S2, electric pulses are used for heating to achieve a heating rate of 350-450°C / min.
4. The heat treatment method of high carbon chromium bearing steel according to claim 3, characterized in that: In step S2, the pulse frequency of the electric pulse is 600-1000 Hz, and the current density is 30-50 A / mm 2 .
5. The heat treatment method of high carbon chromium bearing steel according to claim 1, characterized in that: In step S2, the isothermal austenitizing temperature is 840-860°C, and the holding time is 5-10 minutes.
6. The heat treatment method of high carbon chromium bearing steel according to claim 1 or 5, characterized in that: In step S2, the holding time of the first salt quenching is 10 to 30 minutes; the holding time of the second salt quenching is 20 to 30 minutes.
7. A high carbon chromium bearing steel, characterized in that: The bearing steel is prepared by the heat treatment method of high carbon chromium bearing steel according to any one of claims 1 to 6.
8. The high carbon chromium bearing steel according to claim 7, characterized in that: Calculated in percentage by mass, the high carbon chromium bearing steel consists of the following chemical components: C 0.95%~1.05%, Si 0.15%~0.35%, Mn 0.25%~0.45%, Cr 1.40%~1.65%, Mo≤0.10%, P≤0.025%, S≤0.025%, Ni≤0.30%, Cu≤0.25%, and the remainder is Fe; wherein, Ni+Cu≤0.50%.