Cement mortar prepared using coal gangue material and preparation method thereof
By using materials such as Portland cement, quartz sand, pretreated coal gangue and barium sulfate whisker-modified sodium bentonite in cement mortar, combined with hollow glass beads and supplementary agents, the problem of existing cement mortar is solved. The problem of difficulty in coordinating thermal insulation and crack resistance performance has significantly improved the water resistance and heat resistance stability of the product, and improved the use efficiency.
Patent Information
- Application Number
- CN202410914452.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing cement mortar uses waste coal gangue as the main material. It is difficult to coordinate the thermal insulation and crack resistance properties, and has poor water resistance and heat resistance stability, which limits the efficiency of the product.
Materials such as Portland cement, quartz sand, pre-treated coal gangue, barium sulfate whisker modified sodium bentonite and hollow glass beads are used, combined with supplementary and synergistic agents, to optimize coal through processes such as ultrasonic, heat treatment and ball milling. The activation performance of gangue and the synergistic effect of materials can improve the thermal insulation and crack resistance of the product, and enhance the water resistance and heat resistance stability.
It significantly improves the thermal insulation and crack resistance properties of cement mortar, improves the water resistance and heat resistance stability of the product, and improves usage efficiency.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement mortar, and in particular to a cement mortar prepared by using coal gangue material and a preparation method thereof. Background Art
[0002] Coal gangue is solid waste generated during coal mining and washing, and is an "industrial waste" with solid, liquid and gas hazards. Existing cement mortar uses waste coal gangue as the main material, which can improve the utilization efficiency of coal gangue, but the resulting mortar product has poor thermal insulation and crack resistance. The thermal insulation and crack resistance of the product are difficult to coordinate and improve, and the product has poor water resistance and heat resistance stability, which further limits the use efficiency of the product. Summary of the invention
[0003] In view of the defects of the prior art, the object of the present invention is to provide a cement mortar prepared by using coal gangue material and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] The present invention solves the technical problem by adopting the following technical solution:
[0005] The present invention provides a cement mortar prepared by using coal gangue material, comprising the following raw materials in parts by weight:
[0006] 35-40 parts of Portland cement, 10-15 parts of quartz sand, 10-15 parts of pretreated coal gangue, 8-14 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 8-12 parts of hollow glass microspheres, 4-7 parts of replenishing and improving agent, 3-5 parts of fly ash, 2-4 parts of water reducer, and 40-45 parts of water.
[0007] Preferably, the cement mortar prepared using coal gangue material comprises the following raw materials in parts by weight:
[0008] 37.5 parts of Portland cement, 12.5 parts of quartz sand, 12.5 parts of pretreated coal gangue, 11 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 10 parts of hollow glass microspheres, 5.5 parts of replenishing and improving agent, 4 parts of fly ash, 3 parts of water reducer, and 42.5 parts of water.
[0009] Preferably, the quartz sand is 100 mesh quartz sand; the water reducer is a polycarboxylate water reducer;
[0010] The pretreatment method of pretreatment coal gangue is:
[0011] Place the coal gangue in sufficient water for ultrasonic mixing treatment, with an ultrasonic power of 350~400W and an ultrasonic time of 2h. After the ultrasonic treatment is completed, wash and dry the coal gangue. Heat treat the dried coal gangue at 300℃ for 20~25min. After the treatment is completed, air cool it to room temperature.
[0012] Preferably, the preparation method of the barium sulfate whisker modified sodium bentonite agent is:
[0013] S01: The sodium bentonite is first heat treated at 260-270°C for 5-10 min, then cooled to 155°C at a rate of 1-2°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0014] S02: Preparation of barium sulfate whisker conditioning solution:
[0015] S021: 3-5 parts of barium sulfate whiskers, 1-3 parts of stearic acid, 0.25-0.35 parts of nano-silica sol and 4-7 parts of 5% by mass sodium lignin sulfonate solution are mixed and ball-milled thoroughly at a ball-milling speed of 1000 r / min for 2 hours to obtain a barium sulfate whisker modified solution;
[0016] S022: wollastonite is first treated with proton irradiation at an irradiation power of 350-400 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. 2-5 parts of the irradiated wollastonite are infiltrated into 5-8 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the wollastonite is filtered and dried to obtain a wollastonite regulator.
[0017] S023: Mix and stir 3-5 parts of wollastonite conditioning agent and 4-8 parts of barium sulfate whisker modification liquid, and obtain barium sulfate whisker modification liquid after stirring.
[0018] S03: The sodium bentonite treated with S01 and the barium sulfate whisker conditioning liquid are mixed in a weight ratio of 5:(2~3) and ball-milled at a speed of 1500r / min for 1h. After the ball milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers.
[0019] Preferably, the mass fraction of the sodium citrate solution is 2-5%.
[0020] Preferably, the infiltration power of the ultrasonic infiltration treatment is 350-400 W, and the infiltration time is 20-25 min; the stirring speed of the mixed stirring treatment is 550-650 r / min, and the stirring time is 45-50 min.
[0021] Preferably, the preparation method of the tonic and tonifying agent is:
[0022] S11: preheat the hydroxyapatite at 55-60°C for 5 min, then add it into a 10% sodium silicate solution in a weight ratio of 1:3, stir evenly, then filter and dry;
[0023] S12: The hydroxyapatite and the restoring agent dried in S11 are mixed in a weight ratio of 7:3 and ball-milled at a speed of 1000-1500 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain the restoring agent.
[0024] Preferably, the replenishing and regulating agent comprises the following raw materials in parts by weight:
[0025] 2~5 parts of carboxymethyl cellulose, 1~3 parts of silane coupling agent, 4~6 parts of chitosan solution, 2~4 parts of nano magnesium oxide and 0.25~0.45 parts of 5% by mass sodium aluminate solution.
[0026] Preferably, the silane coupling agent is silane coupling agent KH560; and the mass fraction of the chitosan solution is 2-5%.
[0027] The present invention also provides a method for preparing cement mortar using coal gangue materials, comprising the following steps: weighing cement mortar raw materials according to weight, and stirring and mixing the raw materials in the cement mortar to obtain the cement mortar of the present invention.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The cement mortar of the present invention adopts silicate cement, quartz sand and fly ash to pre-treat coal gangue, and the coal gangue is washed and then improved by heat to optimize its activation performance, and the raw materials of coal gangue are fully utilized. At the same time, hollow glass microspheres are added to improve the thermal insulation effect of the product, and the adjustment agent and the supplementary adjustment agent of the sodium-based bentonite modified by barium sulfate whisker cooperate with each other and work together, so that the thermal insulation and crack resistance of the product are coordinated and improved, and the water resistance and heat resistance stability of the product are remarkable; the adjustment agent of the sodium-based bentonite modified by barium sulfate whisker adopts the sodium-based bentonite that is first heat-treated at 260-270°C for 5-10 min, then cooled to 155°C at a rate of 1-2°C / min, kept warm for 5 min, and finally air-cooled to room temperature to optimize the activity performance and interlamellar spacing of sodium bentonite. Barium sulfate whisker modified liquid was obtained by blending barium sulfate whiskers, stearic acid, nano-silica sol and 5% sodium lignin sulfonate solution with ball milling, and then wollastonite was irradiated with protons to stimulate the activity performance. At the same time, ultrasonic infiltration treatment in sodium citrate solution was used to optimize the activity performance and dispersion of wollastonite. The needle-like structure of wollastonite was combined with barium sulfate whisker modified liquid, and the barium sulfate whisker in the barium sulfate whisker modified liquid was used to prepare the barium sulfate whisker modified liquid. The structure is hybridized with needle-shaped wollastonite. At the same time, the barium sulfate whisker conditioning liquid obtained by blending and adjusting the raw materials in the barium sulfate whisker modification liquid is used to coordinate and improve the sodium-based bentonite. The lamellar sodium-based bentonite interlaced system structure is adopted, and then combined with the barium sulfate whisker conditioning liquid. The co-coordination and synergy between the raw materials are adopted to enhance the thermal insulation and crack resistance of the product, and further enhance the water resistance and heat resistance stability of the product; the hydroxyapatite is preheated at 55-60°C for 5 minutes, and then stirred in a 10% sodium silicate solution by mass. The sodium silicate solution is used to modify the hydroxyapatite. Limestone enhances the stability of hydroxyapatite. At the same time, hydroxyapatite is coordinated in the system in a point structure to enhance the connectivity between the raw materials, thereby reinforcing the performance of the synergistic product. The replenishing and adjusting agent is improved by blending carboxymethyl cellulose, silane coupling agent, chitosan solution, nano-magnesium oxide and 5% by mass sodium aluminate solution. The coordination and synergistic effect of hydroxyapatite is enhanced by coordinating the sodium aluminate solution with nano-magnesium oxide and the raw materials in the coordinating agent. The synergistic effect of the replenishing and adjusting agent and the barium sulfate whisker modified sodium bentonite agent is further enhanced, and the performance of the product is further improved. DETAILED DESCRIPTION
[0030] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The cement mortar prepared from coal gangue material of this embodiment includes the following raw materials in parts by weight:
[0032] 35-40 parts of Portland cement, 10-15 parts of quartz sand, 10-15 parts of pretreated coal gangue, 8-14 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 8-12 parts of hollow glass microspheres, 4-7 parts of replenishing and improving agent, 3-5 parts of fly ash, 2-4 parts of water reducer, and 40-45 parts of water.
[0033] The cement mortar prepared from coal gangue material in this embodiment includes the following raw materials in parts by weight:
[0034] 37.5 parts of Portland cement, 12.5 parts of quartz sand, 12.5 parts of pretreated coal gangue, 11 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 10 parts of hollow glass microspheres, 5.5 parts of replenishing and improving agent, 4 parts of fly ash, 3 parts of water reducer, and 42.5 parts of water.
[0035] The quartz sand in this embodiment is 100 mesh quartz sand; the water reducing agent is a polycarboxylic acid water reducing agent;
[0036] The pretreatment method of pretreatment coal gangue is:
[0037] Place the coal gangue in sufficient water for ultrasonic mixing treatment, with an ultrasonic power of 350~400W and an ultrasonic time of 2h. After the ultrasonic treatment is completed, wash and dry the coal gangue. Heat treat the dried coal gangue at 300℃ for 20~25min. After the treatment is completed, air cool it to room temperature.
[0038] The preparation method of the barium sulfate whisker modified sodium bentonite agent of this embodiment is:
[0039] S01: The sodium bentonite is first heat treated at 260-270°C for 5-10 min, then cooled to 155°C at a rate of 1-2°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0040] S02: Preparation of barium sulfate whisker conditioning solution:
[0041] S021: 3-5 parts of barium sulfate whiskers, 1-3 parts of stearic acid, 0.25-0.35 parts of nano-silica sol and 4-7 parts of 5% by mass sodium lignin sulfonate solution are mixed and ball-milled thoroughly at a ball-milling speed of 1000 r / min for 2 hours to obtain a barium sulfate whisker modified solution;
[0042] S022: wollastonite is first treated with proton irradiation at an irradiation power of 350-400 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. 2-5 parts of the irradiated wollastonite are infiltrated into 5-8 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the wollastonite is filtered and dried to obtain a wollastonite regulator.
[0043] S023: Mix and stir 3-5 parts of wollastonite conditioning agent and 4-8 parts of barium sulfate whisker modification liquid, and obtain barium sulfate whisker modification liquid after stirring.
[0044] S03: The sodium bentonite treated with S01 and the barium sulfate whisker conditioning liquid are mixed in a weight ratio of 5:(2~3) and ball-milled at a speed of 1500r / min for 1h. After the ball milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers.
[0045] The mass fraction of the sodium citrate solution of the present embodiment is 2-5%.
[0046] The infiltration power of the ultrasonic infiltration treatment in this embodiment is 350-400 W, and the infiltration time is 20-25 min; the stirring speed of the mixed stirring treatment is 550-650 r / min, and the stirring time is 45-50 min.
[0047] The preparation method of the tonic and tonifying agent of this embodiment is:
[0048] S11: preheat the hydroxyapatite at 55-60°C for 5 min, then add it into a 10% sodium silicate solution in a weight ratio of 1:3, stir evenly, then filter and dry;
[0049] S12: The hydroxyapatite and the restoring agent dried in S11 are mixed in a weight ratio of 7:3 and ball-milled at a speed of 1000-1500 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain the restoring agent.
[0050] The supplementary effect agent of this embodiment comprises the following raw materials in parts by weight:
[0051] 2~5 parts of carboxymethyl cellulose, 1~3 parts of silane coupling agent, 4~6 parts of chitosan solution, 2~4 parts of nano magnesium oxide and 0.25~0.45 parts of 5% by mass sodium aluminate solution.
[0052] The silane coupling agent of this embodiment is silane coupling agent KH560; the mass fraction of the chitosan solution is 2-5%.
[0053] The method for preparing cement mortar using coal gangue material of the present embodiment comprises the following steps: weighing cement mortar raw materials according to weight, and stirring and mixing the raw materials in the cement mortar to obtain the cement mortar of the present invention.
[0054] Example 1
[0055] The cement mortar prepared from coal gangue material of this embodiment includes the following raw materials in parts by weight:
[0056] 35 parts of silicate cement, 10 parts of quartz sand, 10 parts of pretreated coal gangue, 8 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 8 parts of hollow glass microspheres, 4 parts of replenishing and improving agent, 3 parts of fly ash, 2 parts of water reducer, and 40 parts of water.
[0057] The quartz sand in this embodiment is 100 mesh quartz sand; the water reducing agent is a polycarboxylic acid water reducing agent;
[0058] The pretreatment method of pretreatment coal gangue is:
[0059] Place the coal gangue in sufficient water for ultrasonic mixing treatment. The ultrasonic power is 350W and the ultrasonic time is 2h. After the ultrasonic treatment is completed, wash and dry the dried coal gangue. Heat treat the dried coal gangue at 300℃ for 20min. After the treatment is completed, air cool to room temperature.
[0060] The preparation method of the barium sulfate whisker modified sodium bentonite agent of this embodiment is:
[0061] S01: The sodium bentonite was first heat treated at 260°C for 5 min, then cooled to 155°C at a rate of 1°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0062] S02: Preparation of barium sulfate whisker conditioning solution:
[0063] S021: 3 parts of barium sulfate whiskers, 1 part of stearic acid, 0.25 parts of nano-silica sol and 4 parts of 5% by mass sodium lignin sulfonate solution were mixed and ball-milled thoroughly at a ball-milling speed of 1000 r / min for 2 h to obtain a barium sulfate whisker modified solution;
[0064] S022: Wollastonite is first treated with proton irradiation at an irradiation power of 350 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. Two parts of the irradiated wollastonite are infiltrated into 5 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the solution is filtered and dried to obtain a wollastonite conditioning agent.
[0065] S023: Mix and stir 3 parts of wollastonite conditioning agent and 4 parts of barium sulfate whisker modification liquid, and obtain barium sulfate whisker modification liquid after stirring.
[0066] S03: The sodium bentonite treated with S01 and the barium sulfate whisker conditioning liquid are mixed in a weight ratio of 5:2 and ball-milled at a speed of 1500 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers.
[0067] The mass fraction of the sodium citrate solution in this embodiment is 2%.
[0068] The infiltration power of the ultrasonic infiltration treatment in this embodiment is 350 W, and the infiltration time is 20 min; the stirring speed of the mixed stirring treatment is 550 r / min, and the stirring time is 45 min.
[0069] The preparation method of the tonic and tonifying agent of this embodiment is:
[0070] S11: preheating hydroxyapatite at 55°C for 5 minutes, then adding it into a 10% sodium silicate solution in a weight ratio of 1:3, stirring evenly, and then filtering and drying;
[0071] S12: The hydroxyapatite and the restoring agent dried in S11 are mixed in a weight ratio of 7:3 and ball-milled at a ball-milling speed of 1000 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain the restoring agent.
[0072] The supplementary effect agent of this embodiment comprises the following raw materials in parts by weight:
[0073] 2 parts of carboxymethyl cellulose, 1 part of silane coupling agent, 4 parts of chitosan solution, 2 parts of nano magnesium oxide and 0.25 parts of 5% by mass sodium aluminate solution.
[0074] The silane coupling agent in this embodiment is silane coupling agent KH560; the mass fraction of the chitosan solution is 2%.
[0075] The method for preparing cement mortar using coal gangue material of the present embodiment comprises the following steps: weighing cement mortar raw materials according to weight, and stirring and mixing the raw materials in the cement mortar to obtain the cement mortar of the present invention.
[0076] Example 2
[0077] The cement mortar prepared from coal gangue material of this embodiment includes the following raw materials in parts by weight:
[0078] 40 parts of silicate cement, 15 parts of quartz sand, 15 parts of pretreated coal gangue, 14 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 12 parts of hollow glass microspheres, 7 parts of replenishing and improving agent, 5 parts of fly ash, 4 parts of water reducer, and 45 parts of water.
[0079] The quartz sand in this embodiment is 100 mesh quartz sand; the water reducing agent is a polycarboxylic acid water reducing agent;
[0080] The pretreatment method of pretreatment coal gangue is:
[0081] Place the coal gangue in sufficient water for ultrasonic mixing treatment, with an ultrasonic power of 400 W and an ultrasonic time of 2 h. After the ultrasonic treatment is completed, wash and dry the coal gangue. Heat treat the dried coal gangue at 300 ° C for 25 min. After the treatment is completed, air cool to room temperature.
[0082] The preparation method of the barium sulfate whisker modified sodium bentonite agent of this embodiment is:
[0083] S01: The sodium bentonite was first heat treated at 270°C for 10 min, then cooled to 155°C at a rate of 2°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0084] S02: Preparation of barium sulfate whisker conditioning solution:
[0085] S021: 5 parts of barium sulfate whiskers, 3 parts of stearic acid, 0.35 parts of nano-silica sol and 7 parts of 5% sodium lignin sulfonate solution were mixed and ball-milled at a speed of 1000 r / min for 2 h to obtain a barium sulfate whisker modified solution;
[0086] S022: Wollastonite is first treated with proton irradiation at a power of 400 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. Five parts of the irradiated wollastonite are infiltrated into 8 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the solution is filtered and dried to obtain a wollastonite conditioning agent.
[0087] S023: Mix and stir 5 parts of wollastonite conditioning agent and 8 parts of barium sulfate whisker modification liquid, and obtain barium sulfate whisker modification liquid after stirring.
[0088] S03: The sodium bentonite treated with S01 and the barium sulfate whisker conditioning liquid are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers.
[0089] The mass fraction of the sodium citrate solution in this embodiment is 5%.
[0090] The infiltration power of the ultrasonic infiltration treatment in this embodiment is 400 W, and the infiltration time is 25 min; the stirring speed of the mixed stirring treatment is 650 r / min, and the stirring time is 50 min.
[0091] The preparation method of the tonic and tonifying agent of this embodiment is:
[0092] S11: preheating hydroxyapatite at 60°C for 5 min, then adding it into a 10% sodium silicate solution in a weight ratio of 1:3, stirring evenly, then filtering and drying;
[0093] S12: The hydroxyapatite and the restoring agent dried in S11 are mixed in a weight ratio of 7:3 and ball-milled at a speed of 1500 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain the restoring agent.
[0094] The supplementary effect agent of this embodiment comprises the following raw materials in parts by weight:
[0095] 5 parts of carboxymethyl cellulose, 3 parts of silane coupling agent, 6 parts of chitosan solution, 4 parts of nano magnesium oxide and 0.45 parts of 5% by mass sodium aluminate solution.
[0096] The silane coupling agent in this embodiment is silane coupling agent KH560; the mass fraction of the chitosan solution is 5%.
[0097] The method for preparing cement mortar using coal gangue material of the present embodiment comprises the following steps: weighing cement mortar raw materials according to weight, and stirring and mixing the raw materials in the cement mortar to obtain the cement mortar of the present invention.
[0098] Example 3
[0099] The cement mortar prepared from coal gangue material of this embodiment includes the following raw materials in parts by weight:
[0100] 37.5 parts of Portland cement, 12.5 parts of quartz sand, 12.5 parts of pretreated coal gangue, 11 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 10 parts of hollow glass microspheres, 5.5 parts of replenishing and improving agent, 4 parts of fly ash, 3 parts of water reducer, and 42.5 parts of water.
[0101] The quartz sand in this embodiment is 100 mesh quartz sand; the water reducing agent is a polycarboxylic acid water reducing agent;
[0102] The pretreatment method of pretreatment coal gangue is:
[0103] Place the coal gangue in sufficient water for ultrasonic mixing treatment. The ultrasonic power is 370W and the ultrasonic time is 2h. After the ultrasonic treatment is completed, wash and dry the dried coal gangue. Heat treat the dried coal gangue at 300℃ for 22.5min. After the treatment is completed, air cool to room temperature.
[0104] The preparation method of the barium sulfate whisker modified sodium bentonite agent of this embodiment is:
[0105] S01: The sodium bentonite was first heat treated at 265°C for 7.5 min, then cooled to 155°C at a rate of 1.5°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0106] S02: Preparation of barium sulfate whisker conditioning solution:
[0107] S021: 4 parts of barium sulfate whiskers, 2 parts of stearic acid, 0.30 parts of nano-silica sol and 5.5 parts of 5% sodium lignin sulfonate solution were mixed and ball-milled at a speed of 1000 r / min for 2 h to obtain a barium sulfate whisker modified solution;
[0108] S022: Wollastonite is first treated with proton irradiation at an irradiation power of 370 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. 3.5 parts of the irradiated wollastonite are infiltrated into 6.5 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the solution is filtered and dried to obtain a wollastonite conditioning agent.
[0109] S023: 4 parts of wollastonite conditioning agent and 6 parts of barium sulfate whisker modification liquid are mixed and stirred, and the stirring is completed to obtain a barium sulfate whisker modification liquid;
[0110] S03: The sodium bentonite treated in S01 and the barium sulfate whisker conditioning liquid are mixed in a weight ratio of 2:1 and ball-milled at a speed of 1500 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers.
[0111] The mass fraction of the sodium citrate solution in this embodiment is 3.5%.
[0112] The infiltration power of the ultrasonic infiltration treatment in this embodiment is 375W, and the infiltration time is 22.5min; the stirring speed of the mixed stirring treatment is 600r / min, and the stirring time is 47.5min.
[0113] The preparation method of the tonic and tonifying agent of this embodiment is:
[0114] S11: preheating hydroxyapatite at 57°C for 5 min, then adding it into a 10% sodium silicate solution in a weight ratio of 1:3, stirring evenly, then filtering and drying;
[0115] S12: The hydroxyapatite and the restoring agent dried in S11 are mixed in a weight ratio of 7:3 and ball-milled at a speed of 1250 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain the restoring agent.
[0116] The supplementary effect agent of this embodiment comprises the following raw materials in parts by weight:
[0117] 3.5 parts of carboxymethyl cellulose, 2 parts of silane coupling agent, 5 parts of chitosan solution, 3 parts of nano magnesium oxide and 0.30 parts of 5% by mass sodium aluminate solution.
[0118] The silane coupling agent in this embodiment is silane coupling agent KH560; the mass fraction of the chitosan solution is 3.5%.
[0119] The method for preparing cement mortar using coal gangue material of the present embodiment comprises the following steps: weighing cement mortar raw materials according to weight, and stirring and mixing the raw materials in the cement mortar to obtain the cement mortar of the present invention.
[0120] Comparative Example 1
[0121] The difference from Example 3 is that no barium sulfate whisker-modified sodium bentonite agent is added.
[0122] Comparative Example 2
[0123] The difference from Example 3 is that SO1 treatment is not used in the preparation of the conditioning agent for barium sulfate whisker modified sodium bentonite.
[0124] Comparative Example 3
[0125] The difference from Example 3 is that the barium sulfate whisker conditioning liquid treatment was not used in the preparation of the conditioning agent for the barium sulfate whisker-modified sodium-based bentonite.
[0126] Comparative Example 4
[0127] The difference from Example 3 is that no wollastonite conditioning agent is added to the barium sulfate whisker conditioning solution.
[0128] Comparative Example 5
[0129] The difference from Example 3 is that the wollastonite regulator is replaced by wollastonite.
[0130] Comparative Example 6
[0131] The difference from Example 3 is that no barium sulfate whiskers or nano-silica sol are added to the barium sulfate whisker conditioning solution.
[0132] Comparative Example 7
[0133] The difference from Example 3 is that no tonic agent is added.
[0134] Comparative Example 8
[0135] The difference from Example 3 is that the preparation method of the tonic agent is different: the hydroxyapatite is not treated in step S11.
[0136] Comparative Example 9
[0137] The difference from Example 3 is that the tonic and synergistic agent is not used in the preparation of the tonic and synergistic agent.
[0138] The products of Examples 1 to 3 and Comparative Examples 1 to 9 were subjected to conventional performance tests. The products were immersed in water for 48 hours, and then placed at 70°C for 24 hours. The test was repeated 10 times to test the water immersion and heat resistance stability of the products. The test results are as follows. Table 1 is a test table of thermal conductivity and splitting tensile strength performance under conventional conditions, immersion in water, and heat resistance conditions;
[0139] Table 1:
[0140]
[0141] It can be seen from Comparative Examples 1-9 and Examples 1-3 that;
[0142] The product of Example 3 has excellent thermal insulation performance and excellent splitting tensile strength performance, and the two can be improved in a coordinated manner. In addition, the product has excellent performance stability under water immersion and heat resistance conditions;
[0143] The present invention does not add a barium sulfate whisker modified sodium bentonite adjustment agent or a supplementary adjustment and synergistic agent, and the performance of the product is significantly deteriorated, and the performance stability of the product under water immersion and heat resistance conditions is significantly reduced. The two are used in combination to synergistically enhance the performance of the product, and the performance is significantly improved;
[0144] In the preparation of the barium sulfate whisker modified sodium bentonite adjusting agent, SO1 treatment is not used, barium sulfate whisker conditioning liquid is not used, wollastonite adjusting agent is not added to the barium sulfate whisker conditioning liquid, wollastonite adjusting agent is replaced by wollastonite, barium sulfate whisker and nano-silica sol are not added to the barium sulfate whisker conditioning liquid, and the performance of the product has a tendency to deteriorate. The barium sulfate whisker modified sodium bentonite adjusting agent prepared by using the specific wollastonite adjusting agent of the present invention in combination with the specific barium sulfate whisker conditioning liquid process of the present invention has the most significant product performance effect. The barium sulfate whisker modified sodium bentonite adjusting agent prepared by the specific process steps of the present invention has the most significant product performance effect.
[0145] The preparation methods of the replenishing and conditioning agents are different: the S11 step is not used to treat hydroxyapatite, and the replenishing and conditioning agent is not used in the preparation of the replenishing and conditioning agent. The performance stability of the product under water immersion and heat resistance conditions deteriorates significantly. Only the replenishing and conditioning agent prepared by the method of the present invention has the most significant product performance effect.
[0146] Since the performance of the product is greatly changed by the supplementary agent, further research is conducted on this:
[0147] Comparative Example 10
[0148] The only difference from Example 3 is that no sodium aluminate solution is added to the replenishing agent.
[0149] Comparative Example 11
[0150] The only difference from Example 3 is that the silane coupling agent KH560 is not added to the replenishing agent.
[0151] Comparative Example 12
[0152] The only difference from Example 3 is that no nano magnesium oxide is added to the replenishing agent.
[0153] Comparative Example 13
[0154] The only difference from Example 3 is that the chitosan solution is replaced by deionized water.
[0155] Comparative Example 14
[0156] The only difference from Example 3 is that no carboxymethyl cellulose is added.
[0157] Table 2 is a table showing the effects of the preparation conditions of the supplementary and regulating agent on the product performance. The test results are shown in Table 2;
[0158] Table 2:
[0159]
[0160] It can be seen from Comparative Examples 10-14 that when nano-magnesium oxide is not added in the preparation of the supplementary and regulating agent, the performance of the product deteriorates significantly, followed by the absence of sodium aluminate solution. At the same time, when silane coupling agent KH560 is not added to the supplementary and regulating agent, the chitosan solution is replaced by deionized water, and carboxymethyl cellulose is not added, the performance of the product tends to deteriorate. The chitosan solution, carboxymethyl cellulose, and silane coupling agent KH560 of the present invention are used to prepare nano-magnesium oxide and sodium aluminate solution, and the performance effect of the product is the most significant. Only when the specific raw material formula of the present invention is used, the performance effect of the product is the most significant, and the use of other raw materials instead is not as significant as the effect of the present invention.
[0161] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0162] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A cement mortar prepared using coal gangue material, It is characterized in that It includes the following raw materials in parts by weight: 35-40 parts of Portland cement, 10-15 parts of quartz sand, 10-15 parts of pretreated coal gangue, 8-14 parts of barium sulfate whisker modified sodium bentonite agent, 8-12 parts of hollow glass microspheres, 4-7 parts of replenishing and improving agent, 3-5 parts of fly ash, 2-4 parts of water reducer, 40-45 parts of water; The preparation method of the barium sulfate whisker modified sodium bentonite agent is as follows: S01: The sodium bentonite is first heat treated at 260-270°C for 5-10 min, then cooled to 155°C at a rate of 1-2°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature; S02: Preparation of barium sulfate whisker conditioning solution: S021: 3-5 parts of barium sulfate whiskers, 1-3 parts of stearic acid, 0.25-0.35 parts of nano-silica sol and 4-7 parts of 5% by mass sodium lignin sulfonate solution are mixed and ball-milled thoroughly at a ball-milling speed of 1000 r / min for 2 hours to obtain a barium sulfate whisker modified solution; S022: wollastonite is first treated with proton irradiation at an irradiation power of 350-400 W for 20 minutes. After the irradiation is completed, irradiated wollastonite is obtained. 2-5 parts of the irradiated wollastonite are infiltrated into 5-8 parts of sodium citrate solution for ultrasonic infiltration. After the infiltration is completed, the wollastonite is filtered and dried to obtain a wollastonite regulator. S023: Mix and stir 3-5 parts of wollastonite conditioning agent and 4-8 parts of barium sulfate whisker modification liquid, and obtain barium sulfate whisker modification liquid after stirring. S03: The sodium bentonite treated in S01 and the barium sulfate whisker conditioning liquid are mixed and ball-milled in a weight ratio of 5:(2-3) at a ball-milling speed of 1500r / min for 1h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent for sodium bentonite modified with barium sulfate whiskers; The preparation method of the tonic and tonifying agent is as follows: S11: preheat the hydroxyapatite at 55-60°C for 5 min, then add it into a 10% sodium silicate solution in a weight ratio of 1:3, stir evenly, then filter and dry; S12: mixing the replenishing and regulating agent and the hydroxyapatite dried in S11 in a weight ratio of 3:7, and subjecting the mixture to ball milling treatment. The ball milling speed is 1000-1500 r / min, and the mixture is ball milled for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain the replenishing and regulating agent; The said supplementary and regulating agent comprises the following raw materials in parts by weight: 2~5 parts of carboxymethyl cellulose, 1~3 parts of silane coupling agent, 4~6 parts of chitosan solution, 2~4 parts of nano magnesium oxide and 0.25~0.45 parts of 5% by mass sodium aluminate solution.
2. The cement mortar prepared using coal gangue material according to claim 1, It is characterized in that The cement mortar prepared from coal gangue material comprises the following raw materials in parts by weight: 37.5 parts of Portland cement, 12.5 parts of quartz sand, 12.5 parts of pretreated coal gangue, 11 parts of barium sulfate whisker modified sodium-based bentonite adjustment agent, 10 parts of hollow glass microspheres, 5.5 parts of replenishing and improving agent, 4 parts of fly ash, 3 parts of water reducer, and 42.5 parts of water.
3. The cement mortar prepared from coal gangue material according to claim 1, It is characterized in that The quartz sand is 100 mesh quartz sand; the water reducing agent is polycarboxylate water reducing agent; The pretreatment method of pretreatment coal gangue is: Place the coal gangue in sufficient water for ultrasonic mixing treatment, with an ultrasonic power of 350~400W and an ultrasonic time of 2h. After the ultrasonic treatment is completed, wash and dry the coal gangue. Heat treat the dried coal gangue at 300℃ for 20~25min. After the treatment is completed, air cool it to room temperature.
4. The cement mortar prepared from coal gangue material according to claim 1, It is characterized in that The mass fraction of the sodium citrate solution is 2-5%.
5. The cement mortar prepared using coal gangue material according to claim 1, It is characterized in that The infiltration power of the ultrasonic infiltration treatment is 350-400W, and the infiltration time is 20-25min; the stirring speed of the mixed stirring treatment is 550-650r / min, and the stirring time is 45-50min.
6. The cement mortar prepared from coal gangue material according to claim 1, It is characterized in that The silane coupling agent is silane coupling agent KH560; the mass fraction of the chitosan solution is 2-5%.
7. A method for preparing cement mortar using coal gangue material as claimed in any one of claims 1 to 6, It is characterized in that The following steps are involved: Cement mortar raw materials are weighed according to parts by weight, and the raw materials in the cement mortar are stirred and mixed thoroughly to obtain cement mortar.