A graphene-enhanced carbon-carbon composite material and preparation method thereof
Through chemical vapor deposition method and impregnation treatment of weak acid metal compound solutions, the problems of unstable interface structure and insufficient performance in the preparation of carbon-carbon composite materials are solved, and efficient and short-cycle carbon-carbon composite materials are achieved, with excellent interface Combination and performance.
Patent Information
- Application Number
- CN202410881757.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The existing methods for preparing carbon-carbon composite materials have problems such as long preparation cycle, low production efficiency, serious damage to the carbon fiber surface, unstable interface structure, poor heat transfer and mechanical properties.
Using the preparation method based on chemical vapor deposition method, carbon fibers are impregnated by weak acid metal compound solution to form a uniform graphene layer, and metal catalyst is generated through in-situ reduction to ensure uniform deposition of graphene on the surface and interior of the carbon fiber, and establish stability. The interface combination improves the thermal conductivity path and performance of the material.
Carbon-carbon composite materials with strong interface bonding force, no surface damage to carbon fiber, high production efficiency and excellent material performance are realized, significantly improving their thermal and mechanical properties.
Smart Images

Figure CN118459230B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon-carbon composite materials, and in particular to a graphene-enhanced carbon-carbon composite material and a preparation method thereof. Background Art
[0002] Chemical vapor deposition is a commonly used method for preparing carbon-carbon composite materials. It has the advantages of simple process, easy and precise control, little damage to fibers, and easy to use with other preform densification processes. However, it also has the disadvantages of too long preparation cycle, low production efficiency, and great difficulty in further modifying the obtained composite materials to improve their original performance. In addition, the interface structure of carbon fibers and the connection between interfaces have a great influence on the performance of carbon-carbon composite materials. The method of acid-base etching carbon fibers to enhance surface activity in the prior art will damage the surface structure of carbon fibers to a certain extent. The later deposition process will cause instability in the interface structure of the carbon-carbon composite materials and produce defects such as delamination. In addition, in the presence of defects, the existing carbon-carbon composite material preparation method has no other heat conduction pathways established during the deposition process, resulting in poor thermal conductivity and mechanical properties of the obtained carbon-carbon composite materials. Summary of the invention
[0003] In order to solve the above-mentioned problems of the prior art, the present invention proposes a new method for preparing a carbon-carbon composite material based on chemical vapor deposition and a graphene-enhanced carbon-carbon composite material obtained therefrom. The preparation method can directly use existing chemical vapor deposition equipment and processes to obtain a carbon-carbon composite material with strong interface bonding, no damage to the carbon fiber surface, and a uniform heat conduction path. At the same time, it has high production efficiency and short production cycle. The obtained material has excellent interface performance, convenient modification, and good thermal and mechanical properties.
[0004] The technical solution of the present invention is as follows:
[0005] A method for preparing a graphene-enhanced carbon-carbon composite material, comprising:
[0006] (1) obtaining a weakly acidic metal compound solution;
[0007] (2) fully immersing the carbon fiber preform in the weakly acidic metal compound solution, and then drying to obtain an impregnated preform;
[0008] (3) heating the impregnated preform to 100-300° C. in an inert atmosphere and keeping the temperature for 1-50 hours to obtain a pretreated preform;
[0009] (4) subjecting the pre-treated preform to a chemical vapor deposition reaction in an inert atmosphere and a carbon source gas to obtain a graphene-enhanced carbon-carbon composite material;
[0010] Carrying out chemical vapor deposition reaction in an inert atmosphere and a carbon source gas to obtain a graphene-enhanced carbon-carbon composite material;
[0011] The metal compound solution comprises a first organometallic compound, a second organometallic compound, water and a dispersant for dispersing the first organometallic compound and the second organometallic compound in water, wherein the first organometallic compound is selected from one or more of copper formate, nickel formate, copper acetate and nickel acetate, and the second organometallic compound is selected from amino acid copper and / or copper rosinate.
[0012] The above technical scheme of the present invention carries out an impregnation treatment on the preform through a specific metal compound solution, so that the preform fully absorbs the specific metal compound solution, and in the subsequent heating treatment, the metal catalyst is prepared by in situ synchronous reduction on the surface and inside of the carbon fiber. According to the metal catalyst obtained in situ combined with the control of a specific deposition process, a carbon-carbon composite material with graphene uniformly deposited on the surface and inside of the carbon fiber is prepared.
[0013] In the above technical scheme, the use of a weakly acidic metal compound solution can not only maintain the stability of the metal compound in the solution, but also enhance the bonding strength between the graphene and the carbon fiber matrix in the graphene-reinforced carbon-carbon composite material; the metal compound in the metal compound solution used can be fully adsorbed to the inside and surface of the carbon fiber during the impregnation, and then in situ decomposed during the treatment process of step (3) to form metal and metal oxide, which become catalysts in the chemical vapor deposition reaction, so that graphene with uniform distribution, uniform size and sheet shape is vapor-deposited on the surface and inside of the carbon fiber.
[0014] The inventors unexpectedly discovered that in the above technical scheme, the selection of metal compounds will directly affect whether in-situ grown graphene can be obtained in the subsequent deposition process, as well as the growth quality, distribution uniformity, growth size of the obtained graphene and its interface structure and interface bonding strength with the carbon fiber matrix, etc., and the metal compound solution selected by the present invention can ensure the in-situ growth of high-quality, uniformly distributed, and interface-strongly bonded micron to nanometer-sized graphene in the deposition process through a specific combination of metal compounds, thereby obtaining a graphene-reinforced carbon-carbon composite material with excellent interface performance, convenient modification, and good thermal and mechanical properties.
[0015] In some preferred embodiments, the above steps (1)-(4) can be repeated multiple times to obtain graphene-enhanced carbon-carbon composite materials with different densities according to actual needs. Generally, the more times the above steps (1)-(4) are repeated, the higher the density of the obtained graphene-enhanced carbon-carbon composite material.
[0016] In some preferred embodiments, the preparation method further comprises:
[0017] The graphene-enhanced carbon-carbon composite material is subjected to carbonization and graphitization treatment to obtain a treated graphene-enhanced carbon-carbon composite material.
[0018] Generally, the density of the graphene-reinforced carbon-carbon composite material obtained by the above preferred embodiment is higher than that of the basic graphene-reinforced carbon-carbon composite material that has not been subjected to carbonization and graphitization treatment.
[0019] In some preferred embodiments, the carbonization and graphitization treatment includes: fully pressurizing the graphene-enhanced carbon-carbon composite material into melted asphalt to obtain an asphalt-impregnated material; heating the asphalt-impregnated material at 700-900°C in an inert atmosphere for carbonization to obtain a carbonized material; heating the carbonized material at 2800-3000°C in an inert atmosphere for graphitization to obtain the treated graphene-enhanced carbon-carbon composite material.
[0020] In some preferred embodiments, in the metal compound solution, the concentration of the first organometallic compound is 5-10 mg / L, the concentration of the second organometallic compound is 8-12 mg / L, and the concentration of the dispersant is 1-5 mg / L.
[0021] More preferably, the concentration of the first organometallic compound is 6 mg / L, the concentration of the second organometallic compound is 10 mg / L, and the concentration of the dispersant is 2 mg / L.
[0022] In some preferred embodiments, the dispersant is selected from one or more of polypyrrolidone, stearic acid, citric acid, and sodium octadecyl sulfate.
[0023] The carbon source gas is selected from one or more alkane gases.
[0024] In some preferred embodiments, the chemical vapor deposition reaction includes: heating the pre-treated preform to 800-1100° C., introducing an inert atmosphere gas and the carbon source gas to perform a deposition reaction for 100-300 hours to obtain the graphene-enhanced carbon-carbon composite material.
[0025] In some preferred embodiments, the heating rate is 1-5°C / min.
[0026] In some preferred embodiments, the deposition reaction time is 180-240 hours.
[0027] In some preferred embodiments, the metal compound solution comprises 85 parts by mass of water, 8 parts by mass of copper formate, 11 parts by mass of amino acid copper and / or copper rosinate and 6 parts by mass of a dispersant, and is acidified by hydrochloric acid and / or nitric acid; the inert atmosphere is generated by a mixed gas of Ar and N2, and the carbon source gas is selected from natural gas.
[0028] In some preferred embodiments, the drying temperature is 150-250°C.
[0029] The present invention further provides a graphene-enhanced carbon-carbon composite material prepared according to the above preparation method or a treated graphene-enhanced carbon-carbon composite material obtained by further carbonization and graphitization treatment.
[0030] The obtained graphene-reinforced carbon-carbon composite material contains a carbon fiber matrix, graphene and pyrolytic carbon and / or graphite, wherein the graphene, pyrolytic carbon and / or graphite are all obtained by in-situ reaction on the carbon fiber matrix, and the graphene is in-situ grown on the surface and inside of the carbon fiber matrix, providing a two-phase interface from micrometer scale to nanometer scale for the carbon fiber, pyrolytic carbon and / or graphite, improving the bonding force between different phases of the carbon-carbon composite material, and significantly improving the mechanical properties, thermal properties and electrical properties of the composite material.
[0031] The present invention has the following beneficial effects:
[0032] (1) The preparation method of the present invention has a simple process, high production efficiency, short production cycle, and can be precisely and flexibly controlled;
[0033] (2) The preparation method of the present invention can directly utilize existing chemical vapor deposition equipment and processes, and has good compatibility and strong production capacity;
[0034] (3) In the carbon-carbon composite material obtained by the present invention, graphene grows directly on the surface and inside of the carbon fiber, the interface bonding is firm, and there is no surface damage to the carbon fiber during the preparation process, and the material interface performance is excellent;
[0035] (4) The present invention can obtain graphene-enhanced carbon-carbon composite materials with different performances by adjusting the ratio, concentration, pH value, etc. of the metal compound solution used for preform impregnation, and the modification is convenient;
[0036] (5) The preparation method of the present invention can reduce the metal catalyst in situ, and then prepare the graphene-reinforced carbon-carbon composite material in situ, providing a uniform thermal conductivity path for the obtained carbon-carbon composite material, significantly improving the thermal conductivity of the composite material. At the same time, the micro-nano graphene produced by the present invention can play a filling and reinforcing role in the composite material, so that the obtained carbon-carbon composite material exhibits excellent thermal and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a SEM image of the low-density graphene-reinforced carbon-carbon composite material obtained in Example 1.
[0038] Figure 2 This is a SEM image of the high-density graphene-reinforced carbon-carbon composite material obtained in Example 2.
[0039] Figure 3 This is a SEM image of the low-density carbon-carbon composite material without graphene obtained in Comparative Example 1. DETAILED DESCRIPTION
[0040] The technical scheme of the present invention will be further described below in conjunction with the embodiments and drawings of the present invention. The embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0041] Embodiment 1:
[0042] A low-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0043] (1) adding 8 parts by mass of copper formate, 11 parts by mass of amino acid copper, and 6 parts by mass of polypyrrolidone to 85 parts by mass of pure water in sequence, and after the solids are completely dissolved, adding a small amount of hydrochloric acid or nitric acid to adjust the pH value to 4-5 so that the solution remains weakly acidic, thereby obtaining a saturated solution of the metal compound catalyst;
[0044] (2) Immersing the carbon fiber preform in a saturated solution of a metal compound catalyst for 1 hour to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0045] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0046] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 5°C / min, and then keeping the temperature at 300°C for 1 hour to obtain a pretreated preform;
[0047] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 5°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. Then, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 0.9 g / cm 3 .
[0048] The microstructure of the graphene-enhanced carbon-carbon composite material obtained in step (5) was characterized, and the obtained SEM image is shown in the attached figure. Figure 1 As shown, it can be seen that in this material, graphene is in the form of uniformly sized flakes, which are evenly distributed on the surface of the carbon fiber in situ, and there is no interface stratification between graphene and the carbon fiber.
[0049] Embodiment 2:
[0050] A high-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0051] (1) 8 parts by mass of copper formate, 11 parts by mass of amino acid copper, and 6 parts by mass of polypyrrolidone are added to 85 parts by mass of pure water in sequence. After the solid is completely dissolved, a small amount of hydrochloric acid or nitric acid is added to keep the solution weakly acidic, and a saturated solution of the metal compound catalyst is obtained;
[0052] (2) Immersing the carbon fiber preform in a saturated solution of a metal compound catalyst for 1 hour to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0053] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0054] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 5°C / min, and then keeping the temperature at 300°C for 1 hour to obtain a pretreated preform;
[0055] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 5°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. Then, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 0.9 g / cm 3;
[0056] (6) heating the asphalt at 250° C. in a pressure impregnation container to melt it, and applying pressure to impregnate the melted asphalt into the obtained low-density graphene-reinforced carbon-carbon composite material. After sufficient impregnation, taking out the material and placing it in a carbonization furnace;
[0057] (7) A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the mixture is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the asphalt to obtain a carbonized graphene-reinforced carbon-carbon composite material;
[0058] (8) After the carbonized graphene-enhanced carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density graphene-enhanced carbon-carbon composite material. The density of the material is 1.508 g / cm 3 .
[0059] The high-density graphene-reinforced carbon-carbon composite material obtained in step (8) was characterized microscopically. The obtained SEM image is shown in the attached figure. Figure 2 As shown, it can be seen that in the composite material, the surface of the carbon fiber is covered with a thick new carbon layer, and the voids in the composite material are significantly reduced compared to the preform.
[0060] Embodiment 3:
[0061] A high-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0062] (1) 8 parts by mass of copper formate, 11 parts by mass of amino acid copper, and 6 parts by mass of polypyrrolidone are added to 85 parts by mass of pure water in sequence. After the solid is completely dissolved, a small amount of hydrochloric acid or nitric acid is added to keep the solution weakly acidic, and a saturated solution of the metal compound catalyst is obtained;
[0063] (2) impregnating the carbon fiber preform in a saturated solution of a metal compound catalyst for 5 hours to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0064] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0065] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 1°C / min, and then keeping the temperature at 300°C for 1h to obtain a pretreated preform;
[0066] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 1°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. After that, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 1.1 g / cm 3 ;
[0067] (6) heating the asphalt at 250° C. in a pressure impregnation container to melt it, and applying pressure to impregnate the melted asphalt into the obtained low-density graphene-reinforced carbon-carbon composite material. After sufficient impregnation, taking out the material and placing it in a carbonization furnace;
[0068] (7) A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the mixture is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the asphalt to obtain a carbonized graphene-reinforced carbon-carbon composite material;
[0069] (8) After the carbonized graphene-enhanced carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density graphene-enhanced carbon-carbon composite material. The density of the material is 1.489 g / cm 3 .
[0070] Embodiment 4:
[0071] A high-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0072] (1) 8 parts by mass of copper formate, 11 parts by mass of copper rosinate, and 6 parts by mass of polypyrrolidone are added to 85 parts by mass of pure water in sequence. After the solid is completely dissolved, a small amount of hydrochloric acid or nitric acid is added to keep the solution weakly acidic, thereby obtaining a saturated solution of the metal compound catalyst;
[0073] (2) Immersing the carbon fiber preform in a saturated solution of a metal compound catalyst for 1 hour to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0074] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0075] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 5°C / min, and then keeping the temperature at 300°C for 1 hour to obtain a pretreated preform;
[0076] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 5°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. Then, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 0.85g / cm 3 ;
[0077] (6) heating the asphalt at 250° C. in a pressure impregnation container to melt it, and applying pressure to impregnate the melted asphalt into the obtained low-density graphene-reinforced carbon-carbon composite material. After sufficient impregnation, taking out the material and placing it in a carbonization furnace;
[0078] (7) A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the mixture is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the asphalt to obtain a carbonized graphene-reinforced carbon-carbon composite material;
[0079] (8) After the carbonized graphene-enhanced carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density graphene-enhanced carbon-carbon composite material. The density of the material is 1.412 g / cm 3 .
[0080] Embodiment 5:
[0081] A high-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0082] (1) 8 parts by mass of copper formate, 11 parts by mass of copper rosinate, and 6 parts by mass of sodium dodecyl sulfate are added to 85 parts by mass of pure water in sequence. After the solids are completely dissolved, a small amount of hydrochloric acid or nitric acid is added to keep the solution weakly acidic, thereby obtaining a saturated solution of the metal compound catalyst;
[0083] (2) Immersing the carbon fiber preform in a saturated solution of a metal compound catalyst for 1 hour to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0084] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0085] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 5°C / min, and then keeping the temperature at 300°C for 1 hour to obtain a pretreated preform;
[0086] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 5°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. Then, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 0.85g / cm 3 ;
[0087] (6) heating the asphalt at 250° C. in a pressure impregnation container to melt it, and applying pressure to impregnate the melted asphalt into the obtained low-density graphene-reinforced carbon-carbon composite material. After sufficient impregnation, taking out the material and placing it in a carbonization furnace;
[0088] (7) A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the mixture is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the asphalt to obtain a carbonized graphene-reinforced carbon-carbon composite material;
[0089] (8) After the carbonized graphene-enhanced carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density graphene-enhanced carbon-carbon composite material. The density of the material is 1.406 g / cm 3 .
[0090] Embodiment 6:
[0091] A high-density graphene-reinforced carbon-carbon composite material is prepared by the following steps:
[0092] (1) 8 parts by mass of copper formate, 11 parts by mass of amino acid copper, and 6 parts by mass of polypyrrolidone are added to 85 parts by mass of pure water in sequence. After the solid is completely dissolved, a small amount of hydrochloric acid or nitric acid is added to keep the solution weakly acidic, and a saturated solution of the metal compound catalyst is obtained;
[0093] (2) Immersing the carbon fiber preform in a saturated solution of a metal compound catalyst for 1 hour to allow the impregnation solution to be fully absorbed into the preform to obtain an impregnated preform;
[0094] (3) placing the impregnated preform in a N2-protected oven, heating it at 200°C for 1 hour and then cooling it to room temperature to obtain a dried preform;
[0095] (4) placing the dried preform into a chemical vapor deposition furnace, introducing a mixed gas of Ar and N2 for atmosphere protection, heating from room temperature to 300°C at a heating rate of 5°C / min, and then keeping the temperature at 300°C for 1 hour to obtain a pretreated preform;
[0096] (5) The pre-treated preform in the chemical vapor deposition furnace was heated to 1100°C at a heating rate of 5°C / min, and then a mixed gas of Ar, N2 and natural gas was slowly introduced into the furnace to carry out a chemical vapor deposition reaction. The deposition reaction time was 180 hours. Then, the heating was stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After cooling, the deposition furnace was opened to obtain a low-density graphene-enhanced carbon-carbon composite material. After testing, the density of the material was 0.9 g / cm 3 ;
[0097] (6) transferring the low-density graphene-enhanced carbon-carbon composite material obtained in the previous step to a pressure impregnation container, adding a phenolic resin solution to the pressure impregnation container, and pressurizing the phenolic resin solution to impregnate the obtained low-density graphene-enhanced carbon-carbon composite material. After sufficient impregnation, taking out the material and loading it into a carbonization furnace;
[0098] (7) A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the mixture is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the resin to obtain a carbonized graphene-reinforced carbon-carbon composite material;
[0099] (8) After the carbonized graphene-enhanced carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density graphene-enhanced carbon-carbon composite material. The density of the material is 1.413 g / cm 3 .
[0100] Comparative Example 1:
[0101] The low-density carbon-carbon composite material without graphene was prepared by the following steps:
[0102] The carbon fiber preform was placed in a chemical vapor deposition furnace. Under the protection of a mixed gas of Ar and N2, the temperature was raised from room temperature to 300°C at a heating rate of 5°C / min and kept at that temperature for 1 hour. The temperature was then raised at a heating rate of 5°C / min. After reaching 1100°C, a mixed gas of Ar, N2 and natural gas was slowly introduced to start a chemical vapor deposition reaction. The deposition reaction time was 180 hours. The heating was then stopped, and the introduction of natural gas was stopped at the same time. The mixed gas of Ar and N2 was continued to be introduced to cool the furnace. After sufficient cooling, the deposition furnace was opened to obtain a low-density carbon-carbon composite material without graphene. After testing, its density was 0.9 g / cm 3 .
[0103] The obtained low-density carbon-carbon composite material without graphene was characterized by microstructure, and the obtained SEM image is shown in the attached figure. Figure 3 As shown, it can be seen that in this material, no graphene-like layer structure grows on the surface of the carbon fiber.
[0104] Comparative Example 2:
[0105] The high-density carbon-carbon composite material without graphene was prepared by the following steps:
[0106] (1) placing a carbon fiber preform into a chemical vapor deposition furnace, and under the protection of a mixed gas of Ar and N2, heating the temperature from room temperature to 300°C at a heating rate of 5°C / min and keeping the temperature for 1 hour, and then continuing to heat the temperature at a heating rate of 5°C / min. After reaching 1100°C, slowly introducing a mixed gas of Ar, N2 and natural gas to start a chemical vapor deposition reaction. The deposition reaction time is 180 hours, and then stopping heating and stopping introducing natural gas. Continue to introduce a mixed gas of Ar and N2 to cool the furnace. After sufficient cooling, open the deposition furnace to obtain a low-density carbon-carbon composite material without graphene.
[0107] (2) In a pressure impregnation container, asphalt is heated at 250°C to melt it, and the melted asphalt is pressurized to impregnate the obtained low-density carbon-carbon composite material without graphene. After sufficient impregnation, the material is taken out and placed in a carbonization furnace. A mixed gas of Ar and N2 is introduced into the carbonization furnace for protection, and the asphalt is heated to 800°C for carbonization treatment for 80 hours to fully carbonize the asphalt to obtain a carbon-carbon composite material without graphene reinforcement after carbonization. After the carbonized carbon-carbon composite material is cooled to room temperature, it is transferred to a high-temperature graphitization furnace and heated to 2900°C in an Ar protective atmosphere for high-temperature graphitization for 40 hours. The high-temperature graphitization furnace is then cooled to obtain a high-density carbon-carbon composite material without graphene. After testing, its density is 1.386 g / cm 3 .
[0108] Furthermore, the density, mechanical properties, thermal properties and electrical properties of the graphene-enhanced carbon-carbon composite materials obtained in Examples 2-5 and Comparative Example 2 were tested, wherein the test methods are as follows:
[0109] The bulk density is tested in accordance with GBT 24528-2009 Method for Determination of Bulk Density of Carbon Materials;
[0110] The flexural properties are tested in accordance with GBT 3074.1-2021 Determination of flexural strength of carbon materials;
[0111] The compressive performance is tested in accordance with GBT 1431-2019 Determination of compressive strength of carbon materials;
[0112] Thermal diffusivity is tested in accordance with ASTM E1461-13 (R2022) Standard Test Method for Thermal Diffusivity by Flash Method;
[0113] Thermal conductivity (room temperature) is tested in accordance with GBT 8722-2019 Determination of thermal conductivity of carbon materials;
[0114] The resistivity is tested in accordance with GBT 24525-2009 Method for Determination of Resistivity of Carbon Materials.
[0115] The test results are shown in Table 1 below:
[0116] Table 1 Performance test results
[0117]
[0118] It can be seen that the preparation method of the present invention can in-situ reduce and generate a graphene structural layer with a lamellar structure on the surface and inside of the carbon fiber, and the thermal conductivity, mechanical properties and electrical properties of the obtained composite material are excellent. In particular, the metal compound solution is selected as 8 parts by mass of copper formate, 11 parts by mass of amino acid copper, 6 parts by mass of polypyrrolidone and 85 parts by mass of pure water, the immersion time is 1h, and the heating rate is 5°C / min. The high-density graphene-reinforced carbon-carbon composite material of Example 2 obtained has a high heating rate and a short immersion time, and the mechanical, thermal and electrical properties are better than those of the materials obtained in other embodiments.
[0119] It should be noted that the above is only a preferred embodiment of the present invention, which should not limit the protection scope of the technical solution of the present invention. Any modification of the technical solution recorded in the above embodiments and equivalent replacement of technical features by ordinary technicians in the field within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a graphene-enhanced carbon-carbon composite material, characterized in that: It includes: Obtaining a weakly acidic metal compound solution; Fully immersing the carbon fiber preform in the weakly acidic metal compound solution, and then drying to obtain an impregnated preform; The impregnated preform is heated to 100-300° C. in an inert atmosphere and kept at this temperature for 1-50 hours to obtain a pretreated preform; The pre-treated preform is subjected to a chemical vapor deposition reaction in an inert atmosphere and a carbon source gas to obtain a graphene-enhanced carbon-carbon composite material; The metal compound solution comprises a first organometallic compound, a second organometallic compound, water and a dispersant for dispersing the first organometallic compound and the second organometallic compound in water, wherein the first organometallic compound is selected from one or more of copper formate, nickel formate, copper acetate and nickel acetate, and the second organometallic compound is selected from amino acid copper and / or copper rosinate.
2. The preparation method according to claim 1, characterized in that: It also includes: The graphene-enhanced carbon-carbon composite material is subjected to carbonization and graphitization treatment to obtain a treated graphene-enhanced carbon-carbon composite material.
3. The preparation method according to claim 2, characterized in that: The carbonization and graphitization treatment includes: fully pressurizing and impregnating the graphene-enhanced carbon-carbon composite material into melted asphalt to obtain an asphalt-impregnated material; heating the asphalt-impregnated material at 700-900° C. in an inert atmosphere for carbonization to obtain a carbonized material; heating the carbonized material at 2800-3000° C. in an inert atmosphere for graphitization to obtain the treated graphene-enhanced carbon-carbon composite material.
4. The preparation method according to claim 1, characterized in that: In the metal compound solution, the concentration of the first organic metal compound is 5-10 mg / L, the concentration of the second organic metal compound is 8-12 mg / L, and the concentration of the dispersant is 1-5 mg / L.
5. The preparation method according to claim 1, characterized in that: in, The dispersant is selected from one or more of polypyrrolidone, stearic acid, citric acid, and sodium dodecyl sulfate; and the carbon source gas is selected from one or more of alkane gases.
6. The preparation method according to claim 1, characterized in that: The chemical vapor deposition reaction comprises: heating the pre-treated preform to 800-1100° C., introducing an inert atmosphere gas and the carbon source gas to carry out a deposition reaction for 100-300 hours, and obtaining the graphene-enhanced carbon-carbon composite material.
7. The preparation method according to claim 6, characterized in that: in, The heating rate is 1-5°C / min; the deposition reaction time is 180-240h.
8. The preparation method according to claim 1, characterized in that: The drying temperature is 150-250°C.
9. A graphene-enhanced carbon-carbon composite material prepared according to the preparation method described in any one of claims 1 or 4-8.
10. The treated graphene-reinforced carbon-carbon composite material prepared by the preparation method according to claim 2 or 3.
Citation Information
Patent Citations
Large-scale synthesis method of two-dimensional graphene-like carbon material by using sodium citrate
CN105152167A
Preparation method of graphene-oxide-modified carbon / carbon composite material
CN106684397A