Biodegradable pressure-sensitive adhesive and preparation method thereof

Through the combination of highly crystalline polycaprolactone/polylactic acid composite nanofibers and polylactic acid-amino acid copolymers, the problem of insufficient mechanical properties and viscosity of biodegradable pressure-sensitive adhesives is solved, and its application capabilities in the field of electronic devices are improved. And achieve good biocompatibility and environmental friendliness.

CN118460168BActive Publication Date: 2024-11-29JIANGSU SIRUIDA NEW MATERIAL TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410935183.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Biodegradable pressure-sensitive adhesives have shortcomings in terms of mechanical properties and viscosity, cannot meet the requirements of certain applications, and have poor stability in humid environments.

Method used

The nanofibers were prepared by sonication and electrospinning technology using a combination of highly crystalline polycaprolactone/polylactic acid composite nanofibers, polylactic acid-amino acid copolymers and adhesives to increase the crystallinity and viscosity of the fibers.

Benefits of technology

It significantly improves the mechanical properties and viscosity of biodegradable pressure-sensitive adhesives, enhances its application capabilities in the field of electronic devices, and achieves good biocompatibility and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460168B_ABST
    Figure CN118460168B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of pressure-sensitive adhesives, and provides a biodegradable pressure-sensitive adhesive and a preparation method thereof, wherein the pressure-sensitive adhesive comprises the following components in parts by weight: 5 to 15 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 60 to 140 parts of polylactic acid-amino acid copolymers, 10 to 30 parts of plasticizers, and 20 to 40 parts of adhesives. Preparation method: Each component is weighed by weight, 2 to 10 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers and 10 to 30 parts of plasticizers are mixed in an open mill for 30 to 45 minutes, and then 60 to 140 parts of high-crystalline polylactic acid-amino acid copolymers and 20 to 40 parts of adhesives are added and stirred for 40 to 60 minutes, and each component is fully mixed and uniform. The biodegradable pressure-sensitive adhesive of the present invention has excellent adhesion and peel strength, and has a wide range of application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to a biodegradable pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] Pressure-sensitive adhesives are widely used in the semiconductor field, mainly for bonding and encapsulation of devices. However, traditional pressure-sensitive adhesives may have a negative impact on the performance and stability of semiconductor devices due to the chemical composition of synthetic polymers. In addition, these adhesives may release harmful volatile organic compounds during processing, posing a potential threat to the environment and human health. Therefore, the development of biodegradable pressure-sensitive adhesive materials is crucial. Biodegradable pressure-sensitive adhesives are of great significance for improving the performance and environmental friendliness of semiconductor devices. Compared with traditional synthetic materials, biodegradable pressure-sensitive adhesives are mostly made of natural sources or biodegradable polymers, which have less burden on the environment and less impact on the performance of semiconductor devices. The use of biodegradable pressure-sensitive adhesives can reduce the release of harmful chemicals, thereby reducing the risk of contamination and corrosion to semiconductor devices. After processing, these adhesives can degrade naturally, reducing the burden on the environment. Therefore, the application of biodegradable pressure-sensitive adhesives in the semiconductor field is of great significance. By developing and adopting these materials, we can not only improve the performance and reliability of semiconductor devices, but also reduce the negative impact on the environment and human health. As the demand for environmental sustainability grows, the application of biodegradable pressure-sensitive adhesives in the semiconductor field will become increasingly important.

[0003] Although biodegradable pressure-sensitive adhesive has great potential, it still faces some challenges. First, its degradable pressure-sensitive adhesive has insufficient mechanical resistance and cannot meet the requirements of certain applications. In order to solve this problem, researchers have enhanced the mechanical properties of biodegradable pressure-sensitive adhesive by adding nanofibers. For example, Chinese patent CN116200134A discloses a pressure-sensitive adhesive with cellulose acetate as a reinforcing agent. Although cellulose acetate has certain mechanical properties, its strength and rigidity are relatively low compared with traditional synthetic polymers. In addition, cellulose acetate may absorb moisture and lose strength in a humid environment, which limits its stability and reliability in applications with large humidity changes. Therefore, the mechanical capacity of the current biodegradable pressure-sensitive adhesive needs to be further improved. Secondly, the initial adhesion and holding force of the pressure-sensitive adhesive need to be further improved, and for the protection of electronic products, in addition to requiring good mechanical resistance, it is also necessary to maintain good adhesion with the substrate. Therefore, although biodegradable pressure-sensitive adhesive has the advantages of environmental protection and sustainable development, it still needs to solve the problems of insufficient mechanical properties and viscosity. Summary of the invention

[0004] (1) Technical problems solved

[0005] The purpose of the present invention is to provide a biodegradable pressure-sensitive adhesive and a preparation method thereof, so as to solve the problem that the biodegradable pressure-sensitive adhesive is insufficient in mechanical properties and viscosity.

[0006] (2) Technical solution

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The biodegradable pressure-sensitive adhesive comprises the following components, measured by weight: 5-15 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 60-140 parts of polylactic acid-amino acid copolymer, 10-30 parts of plasticizer and 20-40 parts of adhesive.

[0009] Furthermore, the preparation method of the high-crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: by weight, 10 to 25 parts of 3-aminopropyltriethoxysilane, 20 to 55 parts of polylactic acid nanocellulose and 15 to 25 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 20 to 45 parts of polycaprolactone are added thereto, the mixture is fully stirred and filtered, and then the filtrate is placed in a vacuum drying oven at 40 to 60° C., and after drying, the high-crystalline polycaprolactone / polylactic acid composite nanofiber is obtained.

[0010] Furthermore, the preparation method of polylactic acid nanocellulose is as follows: by weight, 50-80 parts of natural polylactic acid extract, 10-20 parts of bridging agent, and 20-40 parts of chloroform are mixed evenly to obtain a spinning solution for use, and then the polylactic acid nanocellulose is prepared by an electrospinning method. The parameters of the electrospinning are: voltage: 15-20KV, spinning solution supply speed: 3-5ml / h, spinning environment temperature: 50-70°C, and the polylactic acid nanocellulose can be obtained after drying.

[0011] Furthermore, the method for preparing the natural polylactic acid extract is as follows: by weight, 50 to 100 parts of starch and 40 to 60 parts of water are added to a reaction kettle, and then lactobacillus ( Lactobacillus ), fermented at 40-60℃ for 12-24h, and the concentration of lactobacillus was maintained at (2-10) ×10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

[0012] Furthermore, the bridging agent is one of sodium alginate, gelatin and chitosan.

[0013] Furthermore, the preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 40-65 parts of natural polylactic acid extract and 30-50 parts of natural amino acid extract are fully mixed, reacted at 100-150° C. for 60-90 minutes, and the polylactic acid-amino acid copolymer is obtained after natural cooling.

[0014] Furthermore, the preparation method of the natural amino acid extract is as follows: after uniformly mixing 60 to 100 parts of natural protein, 4 to 10 parts of protease and 30 to 60 parts of pure water by weight, heating to 60 to 80° C. for protein decomposition reaction, using hydrochloric acid to maintain the pH range of 3 to 6 during the reaction, and then filtering to obtain the natural amino acid extract.

[0015] Furthermore, the natural protein is one of egg white, milk powder or egg white powder.

[0016] Furthermore, the mass ratio of the natural protein to the protease is (10-15):1.

[0017] Furthermore, the adhesive is rosin resin or natural rubber.

[0018] Furthermore, the plasticizer is one of gelatin, glycerin, soybean oil or honey.

[0019] The present invention also provides a method for preparing a biodegradable pressure-sensitive adhesive, comprising the following steps:

[0020] Weigh each component by weight, mix 2-10 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers and 10-30 parts of plasticizer in an open mixer for 30-45 minutes, then continue to add 60-140 parts of polylactic acid-amino acid copolymer and 20-40 parts of adhesive and continue stirring for 40-60 minutes until all components are fully mixed.

[0021] The purpose of adding a bridging agent in the process of preparing polylactic acid nanocellulose is to improve the crystallinity and mechanical properties of the fiber. The introduction of a bridging agent increases the crosslinking effect between polylactic acid molecular chains, limits the movement of molecular chains, and reduces the distortion and disorderly arrangement of molecular chains. In this way, after electrostatic spinning, the grain distribution inside the polylactic acid nanocellulose is more oriented, and the crystallinity of the fiber is improved. Therefore, the polylactic acid nanocellulose has higher strength and rigidity and can withstand greater stretching, extrusion and shearing force. By improving the crystallinity of the fiber, the mechanical properties of the fiber can be increased, making it more suitable for some application fields with higher strength requirements.

[0022] The present invention combines the advantages of high-crystalline polylactic acid nanocellulose and polycaprolactone when preparing high-crystalline polycaprolactone / polylactic acid composite nanofibers, so as to improve the performance and application scope of the composite nanofibers, particularly in the field of electronic devices. First, by preparing high-crystalline polycaprolactone / polylactic acid composite nanofibers on high-crystalline polylactic acid nanocellulose, the interaction between the two materials and the synergistic effect of crystallization can be achieved. The high-crystalline polylactic acid nanocellulose is used as a template to induce the crystallinity of polycaprolactone during the preparation process. Through the formation and growth of crystal nuclei, polycaprolactone molecules crystallize on a nanoscale and are arranged along an orderly path, thereby improving the crystallinity and regularity of the overall nanofibers. The introduction of this crystal orderliness enables the composite nanofibers to have better mechanical properties and stability. Secondly, the high strength and rigidity of polycaprolactone play a role in enhancing the overall mechanical properties of the fiber in the composite nanofibers. The introduction of polycaprolactone increases the mechanical properties of the composite nanofibers and improves the mechanical strength and reliability of the fiber. At the same time, the good biocompatibility and degradability of polylactic acid bring better biocompatibility and environmental friendliness to the composite nanofibers.

[0023] Compared with conventional polylactic acid, polylactic acid-amino acid copolymers have advantages in improving mechanical properties and viscosity. The introduction of amino acids can significantly improve the strength, stiffness and impact resistance of the copolymers. The side chain structure of amino acids increases the intermolecular interaction force, making the copolymers have higher strength and stiffness, which is suitable for structural materials and engineering applications. At the same time, the introduction of amino acids can increase the energy absorption capacity and impact toughness of the copolymers and improve the impact resistance of the materials. In addition, the viscosity of polylactic acid-amino acid copolymers can be adjusted by regulating the type and proportion of amino acid monomers to meet the requirements of material adhesion and fluidity for different applications. The introduction of amino acids can also enhance the adhesion of copolymers to other materials, making them have better application potential in coatings, bonding and composite materials. In summary, polylactic acid-amino acid copolymers have the advantages of improving mechanical properties and viscosity, providing new possibilities for applications in multiple fields.

[0024] (3) Beneficial technical effects

[0025] The beneficial effects of the present invention are mainly reflected in the following aspects: the present invention improves the crystallinity and mechanical properties of the fiber during the preparation process of polylactic acid nanocellulose by adding a bridging agent. This significantly improves the strength and rigidity of polylactic acid nanocellulose, and it can withstand greater tensile, extrusion and shear forces. This method of enhancing mechanical properties by improving fiber crystallinity makes it more suitable for application fields with high strength requirements. When preparing highly crystalline polycaprolactone / polylactic acid composite nanofibers, the present invention combines the advantages of highly crystalline polylactic acid nanocellulose and polycaprolactone. Polylactic acid nanocellulose is used as a template to induce the crystallinity of polycaprolactone, thereby improving the crystallinity and regularity of the overall nanofibers. The introduction of this crystalline orderliness enables the composite nanofiber to have better mechanical properties and stability. At the same time, the introduction of polycaprolactone increases the tensile, extrusion and shearing resistance of the composite nanofiber, and improves the mechanical strength and reliability of the fiber. In addition, the good biocompatibility and degradability of polylactic acid bring better biocompatibility and environmental friendliness to the composite nanofiber, broadening its application field. The present invention also prepares a polylactic acid-amino acid copolymer by introducing amino acids into polylactic acid. Compared with conventional polylactic acid, the copolymer has advantages in improving mechanical properties and viscosity. The side chain structure of amino acids increases the intermolecular interaction force, so that the copolymer has higher strength, rigidity and impact resistance, and is suitable for structural materials and engineering applications. At the same time, the introduction of amino acids can increase the energy absorption capacity and impact toughness of the copolymer. In addition, by regulating the type and proportion of amino acid monomers, the viscosity of the copolymer can be adjusted to meet the requirements of material adhesion and fluidity for different applications. In summary, the present invention improves the mechanical properties, crystallinity and viscosity of the biodegradable pressure-sensitive adhesive through the synergistic effect between the components, and broadens its application range in the field of electronic devices and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a SEM morphology image of the polylactic acid nanocellulose prepared in Example 1 of the present invention.

[0027] Figure 2 This is the XRD phase diagram of the polylactic acid nanocellulose prepared in Example 1 of the present invention.

[0028] Figure 3 This is a TEM morphology image of the polylactic acid nanocellulose prepared in Example 1 of the present invention.

[0029] Figure 4 This is the XRD phase diagram of the highly crystalline polycaprolactone / polylactic acid composite nanofibers prepared in Example 1 of the present invention.

[0030] Figure 5 This is a TEM morphology image of the highly crystalline polycaprolactone / polylactic acid composite nanofiber prepared in Example 1 of the present invention.

[0031] Figure 6 This is the XRD phase diagram of the polylactic acid nanocellulose prepared in Comparative Example 1 of the present invention.

[0032] Figure 7 This is a fracture morphology diagram of the biodegradable pressure-sensitive adhesive prepared in Example 1 of the present invention after shear failure. DETAILED DESCRIPTION

[0033] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0034] In the case of not specifying specific conditions, the operation in the examples is carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not indicated, are all common products on the market. Parts not mentioned in the technical content of the present invention will be processed with reference to the prior art. Unless otherwise specified, the following examples and comparative examples will be tested in parallel and use the same processing steps and parameters.

[0035] The following table shows the reagents required for the examples and the corresponding purchasing companies.

[0036] Table 1 Reagents required for the examples and comparative examples and the corresponding purchasing companies

[0037]

[0038] Example 1

[0039] The biodegradable pressure-sensitive adhesive comprises the following components, measured by weight: 5 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 60 parts of polylactic acid-amino acid copolymer, 10 parts of plasticizer and 20 parts of adhesive.

[0040] The preparation method of the above-mentioned high-crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: in parts by weight, 10 parts of 3-aminopropyltriethoxysilane, 20 parts of polylactic acid nanocellulose and 15 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 20 parts of polycaprolactone are added thereto, stirred thoroughly and filtered, and then the filtrate is placed in a vacuum drying oven at 40°C. After drying, high-crystalline polycaprolactone / polylactic acid composite nanofibers are obtained.

[0041] The preparation method of the above-mentioned polylactic acid nanocellulose is as follows: by weight, 50 parts of natural polylactic acid extract, 10 parts of bridging agent, and 20 parts of chloroform are mixed evenly to obtain a spinning solution for use, and then the polylactic acid nanocellulose is prepared by an electrospinning method. The parameters of the electrospinning are: voltage: 15KV, spinning solution supply speed: 3ml / h, spinning environment temperature: 50°C, and polylactic acid nanocellulose can be obtained after drying.

[0042] The preparation method of the natural polylactic acid extract is as follows: by weight, 50 parts of starch and 40-60 parts of water are added to a reactor, and then lactobacillus is added and fermented at 40°C for 12 hours. During the fermentation process, the concentration of lactobacillus is maintained at 2×10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

[0043] The above-mentioned bridging agent is sodium alginate.

[0044] The preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 40 parts of natural polylactic acid extract and 30 parts of natural amino acid extract are fully mixed and reacted at 100° C. for 60 minutes, and then the polylactic acid-amino acid copolymer is obtained after natural cooling.

[0045] The preparation method of the above-mentioned natural amino acid extract is as follows: 60 parts of natural protein, 4 parts of protease and 30 parts of pure water are mixed evenly by weight, and then heated to 60°C for protein decomposition reaction. During the reaction, hydrochloric acid is used to maintain the pH range at 3, and then the natural amino acid extract is obtained after filtration.

[0046] The above-mentioned natural protein is egg white.

[0047] The mass ratio of the above-mentioned natural protein to protease is 15:1.

[0048] The above-mentioned adhesive is rosin resin.

[0049] The above plasticizer is gelatin.

[0050] Example 2

[0051] The biodegradable pressure-sensitive adhesive comprises the following components, measured in parts by weight: 8 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 70 parts of polylactic acid-amino acid copolymer, 15 parts of plasticizer and 25 parts of adhesive.

[0052] The preparation method of the above-mentioned high-crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: by weight, 15 parts of 3-aminopropyltriethoxysilane, 25 parts of polylactic acid nanocellulose and 18 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 25 parts of polycaprolactone are added thereto, stirred thoroughly and filtered, and then the filtrate is placed in a vacuum drying oven at 45°C. After drying, high-crystalline polycaprolactone / polylactic acid composite nanofibers are obtained.

[0053] The preparation method of the above-mentioned polylactic acid nanocellulose is as follows: by weight, 60 parts of natural polylactic acid extract, 15 parts of bridging agent, and 25 parts of chloroform are mixed evenly to obtain a spinning solution for use, and then the polylactic acid nanocellulose is prepared by an electrospinning method. The parameters of the electrospinning are: voltage: 16KV, spinning solution supply speed: 3.5ml / h, spinning environment temperature: 55°C, and polylactic acid nanocellulose can be obtained after drying.

[0054] The preparation method of the natural polylactic acid extract is as follows: by weight, 60 parts of starch and 45 parts of water are added to a reactor, and then lactobacillus is added, and fermented at 45°C for 14 hours. During the fermentation process, the concentration of lactobacillus is maintained at 4×10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

[0055] The above-mentioned bridging agent is gelatin.

[0056] The preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 45 parts of natural polylactic acid extract and 35 parts of natural amino acid extract are fully mixed and reacted at 120° C. for 70 minutes, and the polylactic acid-amino acid copolymer is obtained after natural cooling.

[0057] The preparation method of the above-mentioned natural amino acid extract is as follows: 70 parts of natural protein, 7 parts of protease and 40 parts of pure water are mixed evenly by weight, and then heated to 65°C for protein decomposition reaction. During the reaction, hydrochloric acid is used to maintain the pH range at 4, and then the natural amino acid extract is obtained after filtration.

[0058] The above-mentioned natural protein is milk powder.

[0059] The mass ratio of the above natural protein to protease is 10:1.

[0060] The above adhesive is natural rubber.

[0061] The above plasticizer is honey.

[0062] Example 3

[0063] The biodegradable pressure-sensitive adhesive comprises the following components, measured in parts by weight: 12 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 100 parts of polylactic acid-amino acid copolymer, 20 parts of plasticizer and 30 parts of adhesive.

[0064] The preparation method of the above-mentioned high-crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: in parts by weight, 20 parts of 3-aminopropyltriethoxysilane, 40 parts of polylactic acid nanocellulose and 20 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 40 parts of polycaprolactone are added thereto, stirred thoroughly and filtered, and then the filtrate is placed in a vacuum drying oven at 50°C. After drying, high-crystalline polycaprolactone / polylactic acid composite nanofibers are obtained.

[0065] The preparation method of the above-mentioned polylactic acid nanocellulose is as follows: by weight, 60 parts of natural polylactic acid extract, 18 parts of bridging agent, and 35 parts of chloroform are mixed evenly to obtain a spinning solution for use, and then the polylactic acid nanocellulose is prepared by an electrospinning method. The parameters of the electrospinning are: voltage: 18KV, spinning solution supply speed: 4ml / h, spinning environment temperature: 60°C, and polylactic acid nanocellulose can be obtained after drying.

[0066] The preparation method of the natural polylactic acid extract is as follows: 90 parts by weight of starch and 50 parts by weight of water are added to a reactor, and then lactobacillus is added and fermented at 50°C for 20 hours. During the fermentation process, the concentration of lactobacillus is maintained at 8×10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

[0067] The above-mentioned bridging agent is chitosan.

[0068] The preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 58 parts of natural polylactic acid extract and 45 parts of natural amino acid extract are fully mixed and reacted at 120° C. for 80 minutes, and the polylactic acid-amino acid copolymer is obtained after natural cooling.

[0069] The preparation method of the above-mentioned natural amino acid extract is as follows: 90 parts of natural protein, 9 parts of protease and 58 parts of pure water are mixed evenly by weight, heated to 75°C for protein decomposition reaction, and hydrochloric acid is used to maintain the pH range at 5 during the reaction, and then the natural amino acid extract is obtained after filtration.

[0070] The above-mentioned natural protein is protein powder.

[0071] The mass ratio of the above natural protein to protease is 10:1.

[0072] The above adhesive is natural rubber.

[0073] The plasticizer is soybean oil.

[0074] Example 4

[0075] The biodegradable pressure-sensitive adhesive comprises the following components, measured in parts by weight: 15 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers, 140 parts of polylactic acid-amino acid copolymer, 30 parts of plasticizer and 40 parts of adhesive.

[0076] The preparation method of the above-mentioned high-crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: in parts by weight, 25 parts of 3-aminopropyltriethoxysilane, 55 parts of polylactic acid nanocellulose and 25 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 45 parts of polycaprolactone are added thereto, stirred thoroughly and filtered, and then the filtrate is placed in a vacuum drying oven at 60°C. After drying, high-crystalline polycaprolactone / polylactic acid composite nanofibers are obtained.

[0077] The preparation method of the above-mentioned polylactic acid nanocellulose is as follows: by weight, 80 parts of natural polylactic acid extract, 20 parts of bridging agent, and 40 parts of chloroform are mixed evenly to obtain a spinning solution for use, and then the polylactic acid nanocellulose is prepared by an electrospinning method. The parameters of the electrospinning are: voltage: 20KV, spinning solution supply speed: 5ml / h, spinning environment temperature: 70°C, and polylactic acid nanocellulose can be obtained after drying.

[0078] The preparation method of the natural polylactic acid extract is as follows: 100 parts of starch and 60 parts of water are added to a reactor by weight, and then lactobacillus is added to ferment at 60°C for 24 hours. During the fermentation process, the concentration of lactobacillus is maintained at 10×10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

[0079] The above-mentioned bridging agent is chitosan.

[0080] The preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 65 parts of natural polylactic acid extract and 50 parts of natural amino acid extract are fully mixed and reacted at 150° C. for 90 minutes, and the polylactic acid-amino acid copolymer is obtained after natural cooling.

[0081] The preparation method of the above-mentioned natural amino acid extract is as follows: 100 parts of natural protein, 10 parts of protease and 60 parts of pure water are mixed evenly by weight, and then heated to 80°C for protein decomposition reaction. During the reaction, hydrochloric acid is used to maintain the pH range at 6, and then the natural amino acid extract is obtained after filtration.

[0082] The above-mentioned natural protein is protein powder.

[0083] The mass ratio of the above natural protein to protease is 10:1.

[0084] The above adhesive is natural rubber.

[0085] The above plasticizer is honey.

[0086] Example 5

[0087] It is basically the same as Example 1, except that the amount of the high crystalline polycaprolactone / polylactic acid composite nanofiber is 12 parts.

[0088] Comparative Example 1

[0089] It is basically the same as Example 1, except that no bridging agent is added during the preparation of the polylactic acid nanofibers.

[0090] Comparative Example 2

[0091] The method is basically the same as Example 1, except that an equal amount of high-crystalline polycaprolactone / polylactic acid composite nanofibers is replaced by polylactic acid nanocellulose.

[0092] Comparative Example 3

[0093] The method is basically the same as Example 1, except that equal amounts of polylactic acid nanocellulose and polycaprolactone are added separately.

[0094] Comparative Example 4

[0095] The method is substantially the same as Example 1, except that an equal amount of polylactic acid is used to replace the polylactic acid-amino acid copolymer.

[0096] Characterization Tests:

[0097] The present invention uses a scanning electron microscope (SEM) to observe the morphology of polylactic acid nanocellulose. Figure 1 It can be seen that the size of polylactic acid nanocellulose is relatively uniform, the fibers are well dispersed, and the cellulose aspect ratio is relatively high, which provides an excellent structural basis for it to be used as a reinforcing phase for pressure-sensitive adhesives, proving that electrospinning can be used to prepare high-quality polylactic acid nanocellulose. Then XRD was used to analyze the phase of polylactic acid nanocellulose. Figure 2 The XRD spectrum of polylactic acid nanocellulose shows that the XRD spectrum of nanocrystals has a wide spectrum, which is a typical nanocrystal diffraction peak. From the figure, it can be seen that there is only a single polylactic acid phase. Therefore, polylactic acid nanocellulose with excellent crystallization characteristics has good mechanical properties. Figure 3 Transmission electron microscopy (TEM) of polylactic acid nanocellulose shows that the surface of polylactic acid nanocellulose is smooth and free of impurities. Figure 4The XRD spectrum of the highly crystalline polycaprolactone / polylactic acid composite nanofibers shows that in addition to the polylactic acid phase, there is also crystalline polycaprolactone, which proves that the highly crystalline polycaprolactone / polylactic acid composite nanofibers have good crystallinity, which provides good conditions for them to be used as the reinforcing phase of pressure-sensitive adhesives. Figure 5 Transmission electron microscopy (TEM) of highly crystalline polycaprolactone / polylactic acid composite nanofibers shows that polycaprolactone nanoparticles are evenly distributed on the surface of polylactic acid nanocellulose, proving the polycaprolactone / polylactic acid composite microstructure. Figure 6 For the comparative example, the polylactic acid nanocellulose prepared without adding a bridging agent has a very low diffraction peak and few nanocrystals are produced, which proves that the addition of a bridging agent can significantly improve the crystallinity of polylactic acid nanocellulose, thereby improving its mechanical properties. Figure 7 The fracture morphology after the peel strength test of the pressure-sensitive adhesive can be clearly seen. The pull-out of the high-crystalline polycaprolactone / polylactic acid composite nanofibers and the pull-out bridge of the high-crystalline polycaprolactone / polylactic acid composite nanofibers can be inferred to have an impact on the mechanical properties. The formation of pull-out bridges can enhance the bonding strength between the fiber and the matrix, thereby improving the tensile strength and fracture toughness of the composite material.

[0098] Performance Testing:

[0099] Initial tack: According to the provisions of GB / T 4852-2002 "Test Method for Initial Tack of Pressure-Sensitive Adhesive Tapes (Rolling Ball Method)", the maximum size of the steel ball that is stuck to the sticky surface is determined by rolling a standard steel ball over the sticky surface of the adhesive tape sample on the inclined surface. This method can effectively evaluate the initial tack of the adhesive tape. The test process needs to be operated on an inclined glass plate or a hard smooth surface to ensure that the adhesive tape is evenly pasted and free of bubbles. Select a suitable standard steel ball and ensure that its diameter meets the standard requirements. Place the steel ball above the adhesive tape sample so that the bottom of the steel ball is parallel to the sticky surface of the adhesive tape. Release the steel ball and let it roll down the inclined surface, and observe whether it is stuck to the sticky surface of the adhesive tape. If the steel ball is stuck, measure its diameter and record it. The larger the steel ball number, the stronger the initial tack. According to the measured steel ball diameter, the initial tack of the adhesive tape can be evaluated. During the entire testing process, the cleanliness and smoothness of the glass plate or hard smooth surface should be ensured, the relevant standards and regulations should be followed, and the standardization and reliability of the testing process should be ensured.

[0100] 180° peel strength: The test is carried out in accordance with the provisions of GB / T2792. The test process is as follows: The 180° peel strength test is a common method for evaluating the adhesion between materials. The test is carried out in accordance with the provisions of GB / T 2792. The test process includes preparing the specimen, installing the specimen, adjusting the fixture spacing, setting the test speed, starting the test, recording data, calculating the peel strength and analyzing the results. During the test, it is necessary to ensure that the specimen is flat, clean and free of oil, select the appropriate test speed, and accurately record the maximum load and displacement. Finally, the adhesion performance of the material is evaluated by calculating the peel strength and comparing it with the standard value or material performance requirements. Before the test, it should be ensured that the testing machine is in good condition, properly calibrated in accordance with the standard, and follow the operating specifications specified in the standard to ensure the accuracy and reliability of the test results.

[0101] Shear strength: In order to measure the shear strength of the pressure-sensitive adhesive tape, the present invention adopts "GB / T 33332-2016 Test method for dynamic shear strength of adhesive tape" to test the shear strength of the pressure-sensitive adhesive.

[0102] The test of the holding force is carried out in accordance with the provisions of GB / T4851-2014, and the test equipment is CNY-6S holding force tester.

[0103] The test of biodegradability is carried out in accordance with the provisions of GB / T19277.1.

[0104] The initial adhesion, sustained adhesion, 180° peel strength and biodegradability properties of the coatings of Examples 1 to 5 and Comparative Examples 1 to 4 are summarized in Table 2.

[0105] Table 2 Performance of coatings of Examples 1 to 5 and Comparative Examples 1 to 4

[0106]

[0107] The main difference between Example 1 and Comparative Example 1 is whether a bridging agent is added during the preparation of polylactic acid nanocellulose. From Table 2, it can be seen that the addition of a bridging agent can significantly increase the mechanical properties of polylactic acid nanocellulose, so the stickiness resistance and peel strength of Example 1 are significantly better.

[0108] The main difference between Example 1 and Comparative Example 2 is whether polylactic acid nanocellulose or highly crystalline polycaprolactone / polylactic acid composite nanofiber is used. It can be seen that the composite of polycaprolactone and polylactic acid can significantly improve the stickiness resistance and peel strength.

[0109] The main difference between Example 1 and Comparative Example 3 is whether polycaprolactone and polylactic acid are compounded or separated. From Table 2, it can be seen that the compounding of the two can significantly improve the adhesion resistance and peel strength of the pressure-sensitive adhesive, proving that the two have a synergistic relationship.

[0110] The main difference between Example 1 and Comparative Example 3 is whether polylactic acid is copolymerized with amino acid. It can be seen that after the copolymerization, polylactic acid and amino acid undergo esterification and amidation reactions, which increase the adhesion resistance and peel strength of the pressure-sensitive adhesive.

[0111] In summary, the pressure-sensitive adhesive prepared in the present invention has good adhesion resistance and peel strength, and its biodegradability can reach more than 92%, and has wide application value.

[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that all equivalent structural changes made under the concept of the present invention and using the contents of the present invention specification and drawings should be covered within the scope of protection of the claims of the present invention.

Claims

1. The biodegradable pressure-sensitive adhesive comprises the following components in parts by weight: 5-15 parts of high crystalline polycaprolactone / polylactic acid composite nanofibers, 60-140 parts of polylactic acid-amino acid copolymer, 10-30 parts of plasticizer and 20-40 parts of adhesive; The method for preparing the highly crystalline polycaprolactone / polylactic acid composite nanofiber is as follows: by weight, 10 to 25 parts of 3-aminopropyltriethoxysilane, 20 to 55 parts of polylactic acid nanocellulose and 15 to 25 parts of dichloromethane are subjected to ultrasonic treatment to obtain a polylactic acid nanocellulose solution, and then 20 to 45 parts of polycaprolactone are added thereto. After being fully stirred and evenly mixed, the mixture is filtered, and then the filtered matter is placed in a vacuum drying oven at 40-60°C. After drying, highly crystalline polycaprolactone / polylactic acid composite nanofibers are obtained. The preparation method of polylactic acid nanocellulose is as follows: by weight, 50-80 parts of natural polylactic acid extract, 10-20 parts of bridging agent and 20-40 parts of chloroform are mixed evenly to obtain spinning solution for standby use, and then the polylactic acid nanocellulose is prepared by electrospinning method, and the parameters of electrospinning are: voltage: 15-20KV, spinning solution supply speed: 3-5ml / h, spinning environment temperature: 50-70°C, and polylactic acid nanocellulose is obtained after drying; The bridging agent is one of sodium alginate, gelatin and chitosan; The preparation method of the polylactic acid-amino acid copolymer is as follows: by weight, 40-65 parts of natural polylactic acid extract and 30-50 parts of natural amino acid extract are fully mixed, reacted at 100-150° C. for 60-90 minutes, and naturally cooled to obtain the polylactic acid-amino acid copolymer; The preparation method of the natural amino acid extract is as follows: by weight, 60 to 100 parts of natural protein, 4 to 10 parts of protease and 30 to 60 parts of pure water are mixed evenly, and then heated to 60 to 80° C. for protein decomposition reaction. During the reaction, hydrochloric acid is used to maintain the pH range of 3 to 6, and then the natural amino acid extract is obtained after filtration.

2. The biodegradable pressure-sensitive adhesive according to claim 1, characterized in that: The preparation method of the natural polylactic acid extract is as follows: by weight, 50-100 parts of starch and 40-60 parts of water are added to a reactor, and then lactobacillus is added, and fermented at 40-60°C for 12-24 hours. During the fermentation process, the concentration of lactobacillus is maintained at (2-10) × 10 5 CFU / mL, and then the lactobacillus was inactivated by ultraviolet light to obtain the natural polylactic acid extract.

3. The biodegradable pressure-sensitive adhesive according to claim 1, characterized in that: The natural protein is one of egg white, milk powder or egg white powder; The mass ratio of the natural protein to the protease is (10-15):

1.

4. The biodegradable pressure-sensitive adhesive according to claim 1, characterized in that: The adhesive is rosin resin or natural rubber; The plasticizer is one of gelatin, glycerin, soybean oil or honey.

5. The method for preparing the biodegradable pressure-sensitive adhesive according to any one of claims 1 to 4, characterized in that: The following steps are involved: Weigh each component by weight, mix 2-10 parts of high-crystalline polycaprolactone / polylactic acid composite nanofibers and 10-30 parts of plasticizer in an open mixer for 30-45 minutes, then continue to add 60-140 parts of polylactic acid-amino acid copolymer and 20-40 parts of adhesive and continue stirring for 40-60 minutes to fully mix the components.

Citation Information

Patent Citations

  • Degradable plastic pressure-sensitive adhesive tape and preparation method thereof

    CN116200134A

  • Electrostatic spinning method and electrostatic spinning device for preparing nano fiber with one-dimensional order structure

    CN102181948A

  • Method for preparing degradable material modified polylactic acid polymer

    CN104497512A