A puncture-resistant waterproof coiled material and preparation method thereof

By using trichloroacetic acid and chitosan microcapsule technology, as well as a combination of modified calcium carbonate and additives, the problems of insufficient waterproofing and salt-alkali resistance of existing waterproofing membranes have been solved, and efficient root blocking effects and Improved mechanical properties.

CN118461334BActive Publication Date: 2024-10-15WEIFANG SHIHUA CHEM BUILDING MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410924616.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing puncture-resistant waterproofing membranes have problems such as poor waterproofing, poor salt-alkali resistance and low mechanical properties. Especially during high-temperature construction, the root-blocking agent is prone to failure, affecting the root-blocking effect.

Method used

Trichloroacetic acid is used as the root inhibitor, and chitosan microcapsules are prepared to wrap the root inhibitor to maintain stability. It is combined with modified calcium carbonate and specific additives to improve the compatibility and mechanical properties of the asphalt system to prepare a highly efficient Puncture-resistant waterproof membrane.

Benefits of technology

It achieves good waterproof performance, excellent puncture resistance and high-strength mechanical properties of the waterproof membrane. It can remain stable in harsh saline-alkali environments, and the root blocking agent is not easy to fail, which significantly improves the overall performance of the waterproof membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a puncture-resistant waterproof coiled material and a preparation method thereof, belonging to the technical field of waterproof coiled materials; the preparation method comprises preparing root inhibitor particles, modified calcium carbonate, mixing and coating; in the mixing, asphalt and a softener are added and mixed, the temperature is raised to 153-157° C., stirring is performed during the heating process, the stirring speed is 370-382 rpm, the temperature is then raised to 170-174° C., SBS rubber and styrene-butadiene rubber are added, the modified calcium carbonate, root inhibitor particles, antioxidant and auxiliary agent are added after stirring evenly, and then shearing is performed with a high-speed shearing machine, the speed is controlled to be 823-836 rpm, the shearing time is 92-98 min, and after the shearing is completed, a puncture-resistant mixture is obtained; the auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose; the waterproof coiled material prepared by the invention has good puncture resistance, good waterproof performance, high mechanical properties and excellent salt and alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof coiled materials, and in particular relates to a puncture-resistant waterproof coiled material and a preparation method thereof. Background Art

[0002] With the progress of various construction projects, the problem of water leakage on the ground, roof and basement has become increasingly serious. As a result, waterproofing projects have come into being, and various waterproofing materials have emerged one after another. Waterproof membranes have been widely used in building materials and have become one of the important building materials.

[0003] In order to improve living conditions and living environment, roof gardens have become the preferred solution for developers and architects everywhere. However, roof gardens have high requirements for waterproof membranes. They must not only have good waterproof performance, but also be able to prevent plant roots from piercing the waterproof membranes. Traditional waterproof membranes usually enhance their waterproof performance, but do not have anti-root performance. They are easily penetrated by plant root tips, causing building leakage.

[0004] Therefore, the roof garden not only needs to solve the waterproofing problem, but also the problem of plant roots piercing into the waterproof membrane and causing damage to the waterproof membrane.

[0005] At present, there are usually two methods for puncture-resistant waterproof membranes: physical root barrier and chemical root barrier;

[0006] Physical root barrier is to resist the invasion of plant roots at the physical level by enhancing the density and strength of waterproof membranes. However, the root barrier effect of physical root barrier is limited. Gaps are prone to appear at the overlap of waterproof membranes, which allows plant roots to invade the waterproof membranes, resulting in a significant decrease in the waterproof performance of the waterproof membranes.

[0007] The prior art generally adopts a chemical root barrier method, which usually involves adding a chemical root barrier agent to enhance the root barrier performance. However, the chemical root barrier agent is easily ineffective during high-temperature construction, and the chemical root barrier agent is easily migrated with changes in the environment, resulting in poor root barrier effect on plants. There is also the problem of poor compatibility between the chemical root barrier agent and other raw material components of the waterproof membrane, which in turn reduces the mechanical properties.

[0008] CN109440486A discloses a copper-coated glass fiber base asphalt root-penetration-resistant waterproof coiled material, which uses copper-coated glass fiber cloth or copper-coated glass fiber felt prepared from copper-coated glass fiber bundles as the coiled material base, and copper-coated glass fiber as a reinforcing material and a root-blocking agent, thereby improving the high-temperature stability of the waterproof coiled material, avoiding the loss of the root-blocking effect due to high-temperature decomposition during hot-melt welding of asphalt, and improving the tensile strength and tear strength of the waterproof coiled material;

[0009] However, the waterproof roll material prepared by this patent has poor waterproof performance and poor salt and alkali resistance.

[0010] CN114808481A discloses a novel root-proof and puncture-resistant modified asphalt waterproofing coiled material and a preparation method thereof, specifically disclosing that the waterproofing coiled material comprises a modified asphalt coating layer, a base layer and an isolation layer, wherein the material of the modified asphalt coating layer is modified asphalt, and the modified asphalt comprises 10# asphalt, 100# asphalt, cyclohexane oil, a composite root-proof agent, and a filler; wherein the composite root-proof agent is obtained by grafting and polymerizing modified waste rubber powder with the root-proof agent using terephthaloyl peroxide as a high-efficiency initiator, thereby improving the root-proof and puncture-resistant performance and stability of the waterproofing coiled material;

[0011] When modifying asphalt, this patent heats 10# asphalt and 100# asphalt to 150-160℃, adds cyclohexane oil, heats up to 170-180℃, and then adds a composite root inhibitor. At a high temperature of 170-180℃, the composite root inhibitor will partially fail, resulting in a decrease in the root inhibition effect, thereby reducing the root inhibition and puncture resistance of the waterproof membrane. Moreover, the mechanical properties of the waterproof membrane prepared by this method are still low, and the salt and alkali resistance is poor.

[0012] As can be seen from the above, the puncture-resistant waterproof roll prepared by the prior art has the following problems:

[0013] 1. Poor waterproofness and salt and alkali resistance;

[0014] 2. During the preparation process, the root barrier agent is easily ineffective due to high temperature, which in turn affects the root barrier effect;

[0015] 3. Low mechanical properties. Summary of the invention

[0016] In view of the technical problems existing in the prior art, the present invention provides a puncture-resistant waterproof coiled material and a preparation method thereof, which has good waterproof performance, high mechanical properties, excellent salt-alkali resistance, and avoids the problem of high-temperature failure of root inhibitors during the preparation process, and has excellent root inhibition performance.

[0017] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0018] A method for preparing a puncture-resistant waterproof coiled material includes preparing root inhibitor particles, modified calcium carbonate, mixing and coating steps, and the specific operations are as follows:

[0019] 1. Preparation of root inhibitor particles

[0020] (1) Preparation of root inhibitor mixture

[0021] Chitosan was mixed with 0.65-0.69wt% acetic acid solution, heated to 48-52°C at a rate of 0.4-0.6°C / min, and stirred at 48-52°C for 31-37min to obtain a chitosan solution; trichloroacetic acid was mixed with deionized water, heated to 63-68°C at a rate of 1.0-1.4°C / min, and stirred at 63-68°C for 18-23min. After stirring evenly, an emulsifier was added and ultrasonic oscillation treatment was performed. The ultrasonic treatment time was 17-22min. The sound frequency is 20-25kHz, the ultrasonic power is 113-119W, and the root inhibitor solution is obtained after the ultrasonic treatment; the chitosan solution is added to the root inhibitor solution, stirred evenly, and then homogenized, the homogenization time is 2.8-3.2min, the homogenization pressure is 6.0-6.4MPa, the homogenization times are 2 times, after the homogenization is completed, sodium tripolyphosphate is added and stirred, the stirring time is 10-15min, the stirring speed is 338-352rpm, and the stirring is completed to obtain a root inhibitor mixed solution;

[0022] The mass ratio of chitosan to acetic acid solution is 1.1-1.3:100;

[0023] The mass ratio of trichloroacetic acid to deionized water is 5.6-5.8 mg:100 g;

[0024] The mass ratio of deionized water to emulsifier is 85-89:1.9-2.3;

[0025] The emulsifier is a mixture of Tween-80 and sucrose fatty acid ester, and the mass ratio of Tween-80 to sucrose fatty acid ester is 1.6-1.8:1.1-1.3;

[0026] The mass ratio of the chitosan solution, the root inhibitor solution and the sodium tripolyphosphate is 18-20:75-79:0.41-0.45;

[0027] (2) Post-processing

[0028] The root inhibitor mixture is centrifuged, washed, and then pre-cooled for 4.3-4.7 hours at a temperature of -15 to -11°C. After pre-cooling, it is vacuum freeze-dried with a vacuum degree of 60-64Pa and a cold trap temperature of -38 to -34°C for 13-15 hours. After vacuum freeze-drying, it is naturally restored to room temperature to obtain root inhibitor particles.

[0029] 2. Modified calcium carbonate

[0030] (1) Impregnation

[0031] The calcium carbonate is placed in a ball mill for ball milling, the ball milling time is 37-43 minutes, the ball milling speed is 138-145 rpm, the ball-to-material ratio is 4-6:1, and after the ball milling, the ball-milled calcium carbonate is obtained. The ball-milled calcium carbonate is placed in an impregnation liquid of 6-8 times the mass for static treatment, the static time is 17-22 minutes, the static temperature is 59-63° C., the static pressure is 0.07-0.09 MPa, and the calcium carbonate is naturally restored to room temperature after the static treatment. The ball milling treatment is continued in the impregnation liquid, the ball milling speed is 195-206 rpm, the ball milling time is 28-33 minutes, and the ball-to-material ratio is 3-5:1. After the ball milling is completed, the calcium carbonate is dried to obtain the impregnated calcium carbonate;

[0032] The calcium carbonate is heavy calcium carbonate with a particle size of 225-235nm;

[0033] The impregnation liquid is composed of deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether, and the mass ratio of the deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether is 120-125:1.6-1.8:1.0-1.2:1.1-1.3;

[0034] (2) Modification

[0035] The impregnated calcium carbonate is placed in an ethanol solution of 7-9 times the mass, stirred evenly, heated to 50-54°C, and the modified liquid is added, and the addition rate of the modified liquid is controlled to be 0.34-0.36mL / min. After the addition is completed, the temperature is raised to 67-73°C at a rate of 0.3-0.5°C / min, and the stirring is continued. The stirring time is 1.7-1.9h, and the stirring speed is 197-210rpm. After the stirring is completed, the temperature is kept for 18-22min. After the temperature is kept, the modified calcium carbonate is obtained by filtering, washing, and drying.

[0036] The mass concentration of the ethanol solution is 40-44%;

[0037] The mass ratio of the ethanol solution to the modified liquid is 110:1.2-1.4;

[0038] The modified liquid is a mixed liquid of vinyl trimethoxysilane and vinyl tri(β-methoxyethoxy)silane, and the mass ratio of the vinyl trimethoxysilane to the vinyl tri(β-methoxyethoxy)silane is 1.1-1.3:1.

[0039] 3. Mixing

[0040] Add asphalt and softener into the reactor and mix, heat up to 153-157°C, stir continuously during the heating process, the stirring speed is 370-382rpm, then heat up to 170-174°C, add SBS rubber and styrene-butadiene rubber, stir evenly, add modified calcium carbonate, root inhibitor particles, antioxidant and additives, then use a high-speed shearing machine to shear, control the speed to 823-836rpm, and the shearing time to 92-98min. After the high-speed shearing is completed, a puncture-resistant mixture is obtained;

[0041] The mass ratio of the asphalt, softener, SBS rubber, styrene-butadiene rubber, modified calcium carbonate, root inhibitor particles, antioxidant and additive is 100-104:10.2-10.4:7.3-8.1:6.4-7.0:20-24:7.4-7.6:2.0-2.4:2.1-2.5;

[0042] The asphalt is a mixture of 70# asphalt and 100# asphalt, and the mass ratio of the 70# asphalt to the 100# asphalt is 1.4-1.6:1.1-1.3;

[0043] The softener is a combination of paraffin oil and naphthenic oil, and the mass ratio of the paraffin oil to the naphthenic oil is 1.0-1.2:1.6-1.8;

[0044] The antioxidant is a mixture of antioxidant 1098 and antioxidant 1010, and the mass ratio of antioxidant 1098 to antioxidant 1010 is 1.0-1.2:1.2-1.4;

[0045] The auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose, and the mass ratio of the tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose is 2.4-2.6:1.1-1.3:1.5-1.9.

[0046] 4. Coating

[0047] The mixture is conveyed to an oil immersion tank, the tire base is unfolded into the oil immersion tank, and oil coating is performed, and the puncture-resistant mixture is coated on both sides of the tire base, and the coating thickness of the puncture-resistant mixture is 1.6-2.0 mm to obtain a puncture-resistant layer, and polyethylene films are respectively covered on both sides of the puncture-resistant layer, and the thickness of the polyethylene film is 0.14-0.16 mm to form an upper covering layer and a lower covering layer, and after cooling, trimming, and rolling, a puncture-resistant waterproof coiled material is obtained;

[0048] The puncture-resistant waterproof coiled material comprises, from top to bottom, an upper covering layer, an upper surface puncture-resistant layer, a base layer, a lower surface puncture-resistant layer, and a lower covering layer;

[0049] The tire base layer is a polyester fiber non-woven fabric with a thickness of 0.21-0.25 mm.

[0050] A puncture-resistant waterproof coiled material is prepared by the above preparation method.

[0051] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0052] 1. The method for preparing puncture-resistant waterproof coiled material of the present invention adopts trichloroacetic acid as a root inhibitor, which can effectively prevent the growth of plant roots. The present invention adopts chitosan as a wall material, which has good compatibility, stability, controlled release and film-forming properties, and is rich in amino groups. The amino groups and the phosphate groups of sodium tripolyphosphate are electrostatically bonded to solidify the chitosan film to enhance the stability of the chitosan. The present invention encapsulates the root inhibitor in chitosan microcapsules, which can make the root inhibitor less likely to volatilize and become ineffective during heating, and can play a long-term root inhibitor role; and the hydroxyl groups contained on the surface of chitosan can be bonded with the hydroxyl groups in asphalt, thereby making the root inhibitor particles have good binding properties with other components such as asphalt, thereby improving the mechanical properties and stability of the waterproof coiled material, and still maintaining high mechanical properties in a relatively harsh saline-alkali environment;

[0053] The present invention modifies calcium carbonate by first impregnating it, wherein the impregnation liquid is polyethylene glycol and lauryl alcohol polyoxyethylene ether, which can disperse the calcium carbonate, and is combined with ball milling treatment to avoid agglomeration between calcium carbonate particles, and then vinyl silane treatment is performed, thereby reducing the adhesion between calcium carbonate particles and increasing the lipophilicity of the particles. The surface of the modified calcium carbonate is rich in vinyl groups, which can be connected with carboxyl groups in asphalt, improve the compatibility between calcium carbonate and asphalt, increase chemical affinity, and enable calcium carbonate to be uniformly dispersed in the asphalt system, thereby enhancing the interface bonding performance with asphalt, thereby improving the puncture resistance to a certain extent, and combining with specific additives, wherein tributyl citrate is used as a plasticizer, ethylene bisstearamide is used as a lubricant, and hydroxypropyl methylcellulose has film-forming properties, and enables the asphalt mixture to maintain a high viscosity, thereby enhancing the compactness and uniformity of the waterproof coiled material, and combining it with technical means such as specific root inhibitor particles, improves the mechanical properties and mechanical stability of the waterproof coiled material, and has good salt and alkali resistance, good waterproof performance, and excellent puncture resistance.

[0054] 2. The waterproofing membrane prepared by the present invention was tested according to the method of JC / T1075-2008 "Root-penetration-resistant waterproofing membrane for planted roofs", and the test result showed no root penetration;

[0055] 3. The waterproof membrane prepared by the present invention is tested for performance according to GB / T 328-2007 "Test Methods for Building Waterproof Membrane", with a tensile force of 558-596N / 50mm, an elongation at break of 430-438%, a seam peel strength of 3.69-3.78N / mm, a water impermeability of 0.6MPa, and is water impermeable within 54-60min. The heat resistance is 135-138°C without flowing, bubbling or sliding;

[0056] 4. The waterproof coiled material prepared by the present invention is first soaked in a 21wt% sodium hydroxide solution for 4 days, washed and dried, and then soaked in a 20wt% sodium chloride solution for 4 days, washed and dried. The tensile force is measured to be 541-556N / 50mm, the elongation at break is 418-429%, and the seam peel strength is 3.54-3.66N / mm. DETAILED DESCRIPTION

[0057] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0058] Example 1

[0059] 1. Preparation of root inhibitor particles

[0060] (1) Preparation of root inhibitor mixture

[0061] Chitosan was mixed with 0.67wt% acetic acid solution, heated to 50℃ at a rate of 0.5℃ / min, stirred at 50℃ for 34min to obtain chitosan solution; trichloroacetic acid was mixed with deionized water, heated to 66℃ at a rate of 1.2℃ / min, stirred at 66℃ for 20min, and after stirring evenly, an emulsifier was added for ultrasonic oscillation treatment, the ultrasonic treatment time was 20min, the ultrasonic frequency was 23kHz, the ultrasonic power was 116W, and a root inhibitor solution was obtained after the ultrasonic treatment; the chitosan solution was added to the root inhibitor solution, stirred evenly, and then homogenized, the homogenization time was 3min, the homogenization pressure was 6.2MPa, the homogenization times were 2 times, after the homogenization was completed, sodium tripolyphosphate was added for stirring, the stirring time was 13min, the stirring speed was 347rpm, and the stirring was completed to obtain a root inhibitor mixed solution;

[0062] The mass ratio of chitosan to acetic acid solution is 1.2:100;

[0063] The mass ratio of trichloroacetic acid to deionized water is 5.7 mg:100 g;

[0064] The mass ratio of deionized water to emulsifier is 87:2.1;

[0065] The emulsifier is a mixture of Tween-80 and sucrose fatty acid ester, and the mass ratio of Tween-80 to sucrose fatty acid ester is 1.7:1.2;

[0066] The mass ratio of the chitosan solution, the root inhibitor solution and the sodium tripolyphosphate is 19:77:0.43;

[0067] (2) Post-processing

[0068] The root inhibitor mixture was centrifuged, washed, and then pre-cooled for 4.5 hours at a temperature of -13°C. After pre-cooling, it was vacuum freeze-dried with a vacuum degree of 62 Pa and a cold trap temperature of -36°C for 14 hours. After vacuum freeze-drying, it was naturally restored to room temperature to obtain root inhibitor particles.

[0069] 2. Modified calcium carbonate

[0070] (1) Impregnation

[0071] The calcium carbonate was placed in a ball mill for ball milling, the ball milling time was 40 minutes, the ball milling speed was 142 rpm, the ball-to-material ratio was 5:1, and after the ball milling, the ball-milled calcium carbonate was obtained. The ball-milled calcium carbonate was placed in an impregnation liquid of 7 times the mass for static treatment, the static time was 20 minutes, the static temperature was 61°C, the static pressure was 0.08 MPa, and the calcium carbonate naturally returned to room temperature after the static treatment. The ball milling was continued in the impregnation liquid, the ball milling speed was 201 rpm, the ball milling time was 31 minutes, and the ball-to-material ratio was 4:1. After the ball milling was completed, the calcium carbonate was dried to obtain the impregnated calcium carbonate.

[0072] The calcium carbonate is heavy calcium carbonate with a particle size of 230 nm;

[0073] The impregnation liquid is composed of deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether, and the mass ratio of the deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether is 123:1.7:1.1:1.2;

[0074] (2) Modification

[0075] The impregnated calcium carbonate was placed in an ethanol solution of 8 times its mass, stirred evenly, heated to 52°C, and the modified liquid was added, and the addition rate of the modified liquid was controlled to be 0.35 mL / min. After the addition was completed, the temperature was raised to 71°C at a rate of 0.4°C / min, and the stirring was continued. The stirring time was 1.8 hours, and the stirring speed was 203 rpm. After the stirring was completed, the temperature was kept for 20 minutes. After the temperature was finished, the modified calcium carbonate was obtained by filtering, washing, and drying.

[0076] The mass concentration of the ethanol solution is 42%;

[0077] The mass ratio of the ethanol solution to the modified liquid is 110:1.3;

[0078] The modified liquid is a mixed liquid of vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane, and the mass ratio of the vinyl trimethoxy silane to the vinyl tri (β-methoxyethoxy) silane is 1.2:1.

[0079] 3. Mixing

[0080] Asphalt and softener are added to a reactor and mixed, and the temperature is raised to 155°C. Stirring is continued during the heating process, and the stirring speed is 376 rpm. Then the temperature is raised to 172°C, SBS rubber and styrene-butadiene rubber are added, and after stirring evenly, modified calcium carbonate, root inhibitor particles, antioxidants and additives are added. Then, a high-speed shearing machine is used for shearing, and the speed is controlled to be 830 rpm. The shearing time is 95 minutes. After the high-speed shearing is completed, a puncture-resistant mixture is obtained;

[0081] The mass ratio of the asphalt, softener, SBS rubber, styrene-butadiene rubber, modified calcium carbonate, root inhibitor particles, antioxidant and additive is 102:10.3:7.8:6.7:22:7.5:2.2:2.3;

[0082] The asphalt is a mixture of 70# asphalt and 100# asphalt, and the mass ratio of the 70# asphalt to the 100# asphalt is 1.5:1.2;

[0083] The softener is a combination of paraffin oil and naphthenic oil, and the mass ratio of the paraffin oil to the naphthenic oil is 1.1:1.7;

[0084] The antioxidant is a mixture of antioxidant 1098 and antioxidant 1010, and the mass ratio of antioxidant 1098 to antioxidant 1010 is 1.1:1.3;

[0085] The auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose, and the mass ratio of the tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose is 2.5:1.2:1.7.

[0086] 4. Coating

[0087] The mixture is conveyed to an oil immersion tank, the tire base is unfolded into the oil immersion tank, and oil coating is performed, and the puncture-resistant mixture is coated on both sides of the tire base, and the coating thickness of the puncture-resistant mixture is 1.8 mm to obtain a puncture-resistant layer, and polyethylene films are respectively covered on both sides of the puncture-resistant layer, and the thickness of the polyethylene film is 0.15 mm to form an upper covering layer and a lower covering layer, and after cooling, trimming, and rolling, a puncture-resistant waterproof coiled material is obtained;

[0088] The puncture-resistant waterproof coiled material comprises, from top to bottom, an upper covering layer, an upper surface puncture-resistant layer, a base layer, a lower surface puncture-resistant layer, and a lower covering layer;

[0089] The tire base layer is a polyester fiber non-woven fabric with a thickness of 0.23 mm.

[0090] Example 2

[0091] 1. Preparation of root inhibitor particles

[0092] (1) Preparation of root inhibitor mixture

[0093] Chitosan was mixed with 0.65wt% acetic acid solution, heated to 48°C at a rate of 0.4°C / min, stirred at 48°C for 31min to obtain a chitosan solution; trichloroacetic acid was mixed with deionized water, heated to 63°C at a rate of 1.0°C / min, stirred at 63°C for 18min, and after stirring evenly, an emulsifier was added for ultrasonic oscillation treatment, the ultrasonic treatment time was 17min, the ultrasonic frequency was 20kHz, the ultrasonic power was 113W, and a root inhibitor solution was obtained after the ultrasonic treatment was completed; the chitosan solution was added to the root inhibitor solution, stirred evenly, and then homogenized, the homogenization time was 2.8min, the homogenization pressure was 6.0MPa, the homogenization times were 2 times, after the homogenization was completed, sodium tripolyphosphate was added for stirring, the stirring time was 10min, the stirring speed was 338rpm, and the stirring was completed to obtain a root inhibitor mixed solution;

[0094] The mass ratio of chitosan to acetic acid solution is 1.1:100;

[0095] The mass ratio of trichloroacetic acid to deionized water is 5.6 mg:100 g;

[0096] The mass ratio of deionized water to emulsifier is 85:1.9;

[0097] The emulsifier is a mixture of Tween-80 and sucrose fatty acid ester, and the mass ratio of Tween-80 to sucrose fatty acid ester is 1.6:1.1;

[0098] The mass ratio of the chitosan solution, the root inhibitor solution and the sodium tripolyphosphate is 18:75:0.41;

[0099] (2) Post-processing

[0100] The root inhibitor mixture was centrifuged, washed, and then pre-cooled for 4.3 hours at a temperature of -11°C. After pre-cooling, it was vacuum freeze-dried with a vacuum degree of 60 Pa and a cold trap temperature of -34°C for 13 hours. After vacuum freeze-drying, it was naturally restored to room temperature to obtain root inhibitor particles.

[0101] 2. Modified calcium carbonate

[0102] (1) Impregnation

[0103] The calcium carbonate was placed in a ball mill for ball milling, the ball milling time was 37 minutes, the ball milling speed was 138 rpm, the ball-to-material ratio was 4:1, and after the ball milling, the ball-milled calcium carbonate was obtained. The ball-milled calcium carbonate was placed in an impregnation liquid of 6 times the mass for static treatment, the static time was 17 minutes, the static temperature was 59°C, the static pressure was 0.07 MPa, and the temperature was naturally restored to room temperature after the static treatment. The ball milling was continued in the impregnation liquid, the ball milling speed was 195 rpm, the ball milling time was 28 minutes, and the ball-to-material ratio was 3:1. After the ball milling was completed, the calcium carbonate was dried to obtain the impregnated calcium carbonate;

[0104] The calcium carbonate is heavy calcium carbonate with a particle size of 225 nm;

[0105] The impregnation liquid is composed of deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether, and the mass ratio of the deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether is 120:1.6:1.0:1.1;

[0106] (2) Modification

[0107] The impregnated calcium carbonate was placed in an ethanol solution of 7 times its mass, stirred evenly, heated to 50°C, and the modified liquid was added, and the addition rate of the modified liquid was controlled to be 0.34mL / min. After the addition was completed, the temperature was raised to 67°C at a rate of 0.3°C / min, and the stirring was continued. The stirring time was 1.7h and the stirring speed was 197rpm. After the stirring was completed, the solution was kept warm for 18min. After the heat preservation was completed, the solution was filtered, washed, and dried to obtain modified calcium carbonate;

[0108] The mass concentration of the ethanol solution is 40%;

[0109] The mass ratio of the ethanol solution to the modified liquid is 110:1.2;

[0110] The modified liquid is a mixed liquid of vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane, and the mass ratio of the vinyl trimethoxy silane to the vinyl tri (β-methoxyethoxy) silane is 1.1:1.

[0111] 3. Mixing

[0112] Asphalt and softener are added to a reactor and mixed, and the temperature is raised to 153°C. Stirring is continued during the heating process, and the stirring speed is 370 rpm. Then the temperature is raised to 170°C, SBS rubber and styrene-butadiene rubber are added, and after stirring evenly, modified calcium carbonate, root inhibitor particles, antioxidants and additives are added. Then, a high-speed shearing machine is used for shearing, and the speed is controlled to be 823 rpm. The shearing time is 92 minutes. After the high-speed shearing is completed, a puncture-resistant mixture is obtained;

[0113] The mass ratio of the asphalt, softener, SBS rubber, styrene-butadiene rubber, modified calcium carbonate, root inhibitor particles, antioxidant and additive is 100:10.2:7.3:6.4:20:7.4:2.0:2.1;

[0114] The asphalt is a mixture of 70# asphalt and 100# asphalt, and the mass ratio of the 70# asphalt to the 100# asphalt is 1.4:1.1;

[0115] The softener is a combination of paraffin oil and naphthenic oil, and the mass ratio of the paraffin oil to the naphthenic oil is 1.0:1.6;

[0116] The antioxidant is a mixture of antioxidant 1098 and antioxidant 1010, and the mass ratio of antioxidant 1098 to antioxidant 1010 is 1.0:1.2;

[0117] The auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose, and the mass ratio of the tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose is 2.4:1.1:1.5.

[0118] 4. Coating

[0119] The mixture is conveyed to an oil immersion tank, the tire base is unfolded into the oil immersion tank, and oil coating is performed, and the puncture-resistant mixture is coated on both sides of the tire base, and the coating thickness of the puncture-resistant mixture is 1.6 mm to obtain a puncture-resistant layer, and polyethylene films are respectively covered on both sides of the puncture-resistant layer, and the thickness of the polyethylene film is 0.14 mm to form an upper covering layer and a lower covering layer, and after cooling, trimming, and rolling, a puncture-resistant waterproof coiled material is obtained;

[0120] The puncture-resistant waterproof coiled material comprises, from top to bottom, an upper covering layer, an upper surface puncture-resistant layer, a base layer, a lower surface puncture-resistant layer, and a lower covering layer;

[0121] The tire base layer is a polyester fiber non-woven fabric with a thickness of 0.21 mm.

[0122] Example 3

[0123] 1. Preparation of root inhibitor particles

[0124] (1) Preparation of root inhibitor mixture

[0125] Chitosan was mixed with 0.69wt% acetic acid solution, heated to 52°C at a rate of 0.6°C / min, and stirred at 52°C for 37min to obtain a chitosan solution; trichloroacetic acid was mixed with deionized water, heated to 68°C at a rate of 1.4°C / min, and stirred at 68°C for 23min. After stirring evenly, an emulsifier was added for ultrasonic oscillation treatment. The ultrasonic treatment time was 22min, the ultrasonic frequency was 25kHz, and the ultrasonic power was 119W. After the ultrasonic treatment, a root inhibitor solution was obtained; the chitosan solution was added to the root inhibitor solution, stirred evenly, and then homogenized. The homogenization time was 3.2min, the homogenization pressure was 6.4MPa, and the homogenization times were 2 times. After the homogenization was completed, sodium tripolyphosphate was added for stirring. The stirring time was 15min and the stirring speed was 352rpm. After the stirring was completed, a root inhibitor mixed solution was obtained;

[0126] The mass ratio of chitosan to acetic acid solution is 1.3:100;

[0127] The mass ratio of trichloroacetic acid to deionized water is 5.8 mg:100 g;

[0128] The mass ratio of deionized water to emulsifier is 89:2.3;

[0129] The emulsifier is a mixture of Tween-80 and sucrose fatty acid ester, and the mass ratio of Tween-80 to sucrose fatty acid ester is 1.8:1.3;

[0130] The mass ratio of the chitosan solution, the root inhibitor solution and the sodium tripolyphosphate is 20:79:0.45;

[0131] (2) Post-processing

[0132] The root inhibitor mixture was centrifuged, washed, and then pre-cooled for 4.7 hours at a temperature of -15°C. After pre-cooling, it was vacuum freeze-dried with a vacuum degree of 64 Pa and a cold trap temperature of -38°C for 15 hours. After vacuum freeze-drying, it was naturally restored to room temperature to obtain root inhibitor particles.

[0133] 2. Modified calcium carbonate

[0134] (1) Impregnation

[0135] The calcium carbonate was placed in a ball mill for ball milling, the ball milling time was 43 minutes, the ball milling speed was 145 rpm, the ball-to-material ratio was 6:1, and after the ball milling, the ball-milled calcium carbonate was obtained. The ball-milled calcium carbonate was placed in an impregnation liquid of 8 times the mass for static treatment, the static time was 22 minutes, the static temperature was 63°C, the static pressure was 0.09 MPa, and the temperature was naturally restored to room temperature after the static treatment. The ball milling was continued in the impregnation liquid, the ball milling speed was 206 rpm, the ball milling time was 33 minutes, and the ball-to-material ratio was 5:1. After the ball milling was completed, the calcium carbonate was dried to obtain the impregnated calcium carbonate;

[0136] The calcium carbonate is heavy calcium carbonate with a particle size of 235 nm;

[0137] The impregnation liquid is composed of deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether, and the mass ratio of the deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether is 125:1.8:1.2:1.3;

[0138] (2) Modification

[0139] The impregnated calcium carbonate was placed in an ethanol solution of 9 times its mass, stirred evenly, heated to 54°C, and the modified liquid was added, and the addition rate of the modified liquid was controlled to be 0.36mL / min. After the addition was completed, the temperature was raised to 73°C at a rate of 0.5°C / min, and the stirring was continued. The stirring time was 1.9h and the stirring speed was 210rpm. After the stirring was completed, the solution was kept warm for 22min. After the heat preservation was completed, the solution was filtered, washed, and dried to obtain modified calcium carbonate;

[0140] The mass concentration of the ethanol solution is 44%;

[0141] The mass ratio of the ethanol solution to the modified liquid is 110:1.4;

[0142] The modified liquid is a mixed liquid of vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane, and the mass ratio of the vinyl trimethoxy silane to the vinyl tri (β-methoxyethoxy) silane is 1.3:1.

[0143] 3. Mixing

[0144] Asphalt and softener are added to a reactor and mixed, and the temperature is raised to 157°C. Stirring is continued during the heating process, and the stirring speed is 382 rpm. Then the temperature is raised to 174°C, SBS rubber and styrene-butadiene rubber are added, and after stirring evenly, modified calcium carbonate, root inhibitor particles, antioxidants and additives are added. Then, a high-speed shearing machine is used for shearing, and the speed is controlled to be 836 rpm. The shearing time is 98 minutes. After the high-speed shearing is completed, a puncture-resistant mixture is obtained;

[0145] The mass ratio of the asphalt, softener, SBS rubber, styrene-butadiene rubber, modified calcium carbonate, root inhibitor particles, antioxidant and additive is 104:10.4:8.1:7.0:24:7.6:2.4:2.5;

[0146] The asphalt is a mixture of 70# asphalt and 100# asphalt, and the mass ratio of the 70# asphalt to the 100# asphalt is 1.6:1.3;

[0147] The softener is a combination of paraffin oil and naphthenic oil, and the mass ratio of the paraffin oil to the naphthenic oil is 1.2:1.8;

[0148] The antioxidant is a mixture of antioxidant 1098 and antioxidant 1010, and the mass ratio of antioxidant 1098 to antioxidant 1010 is 1.2:1.4;

[0149] The auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose, and the mass ratio of the tributyl citrate, ethylene bisstearamide and hydroxypropyl methylcellulose is 2.6:1.3:1.9.

[0150] 4. Coating

[0151] The mixture is conveyed to an oil immersion tank, the tire base is unfolded into the oil immersion tank, and oil coating is performed, and the puncture-resistant mixture is coated on both sides of the tire base, and the coating thickness of the puncture-resistant mixture is 2.0 mm to obtain a puncture-resistant layer, and polyethylene films are respectively covered on both sides of the puncture-resistant layer, and the thickness of the polyethylene film is 0.16 mm to form an upper covering layer and a lower covering layer, and after cooling, trimming, and rolling, a puncture-resistant waterproof coiled material is obtained;

[0152] The puncture-resistant waterproof coiled material comprises, from top to bottom, an upper covering layer, an upper surface puncture-resistant layer, a base layer, a lower surface puncture-resistant layer, and a lower covering layer;

[0153] The tire base layer is a polyester fiber non-woven fabric with a thickness of 0.25 mm.

[0154] Comparative Example 1

[0155] Based on Example 1, the changes are that the preparation of the root inhibitor particles is omitted, and the root inhibitor particles are replaced with trichloroacetic acid in an equal amount in the mixing step, and the other operations are the same.

[0156] Comparative Example 2

[0157] Based on Example 1, the changes are as follows:

[0158] ① The modified calcium carbonate step is omitted, and in the mixing step, an equal amount of the modified calcium carbonate is replaced by calcium carbonate;

[0159] ②Omit the auxiliary ingredients in the mixing step;

[0160] The rest of the operations are the same.

[0161] Performance Testing

[0162] The products of Examples 1-3 and Comparative Examples 1-2 were subjected to the following performance tests, as follows:

[0163] 1. Puncture resistance

[0164] The waterproof membranes prepared in Examples 1-3 and Comparative Examples 1-2 were tested according to the method of JC / T1075-2008 "Root-penetration-resistant waterproof membranes for planted roofs". The test results are as follows:

[0165]

[0166] 2. Other performance

[0167] The waterproof membranes prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests according to GB / T 328-2007 "Test Methods for Building Waterproof Membrane", and the test results are as follows:

[0168]

[0169] 3. Salt and alkali resistance

[0170] The waterproof membranes prepared in Examples 1-3 and Comparative Examples 1-2 were first immersed in a 21wt% sodium hydroxide solution for 4 days, washed and dried, immersed in a 20wt% sodium chloride solution for 4 days, washed and dried, and then again tested for performance according to GB / T 328-2007 "Test Methods for Building Waterproof Membrane". The test results are as follows:

[0171]

[0172] The present invention adopts trichloroacetic acid as a root inhibitor, which can effectively prevent the growth of plant roots. The present invention adopts chitosan as a wall material, which has good compatibility, stability, controlled release and film-forming properties, and is rich in amino groups. The amino groups and the phosphate groups of sodium tripolyphosphate are electrostatically bonded to solidify the chitosan film and enhance the stability of the chitosan. The present invention encapsulates the root inhibitor in chitosan microcapsules, which can make the root inhibitor less likely to volatilize and become ineffective during heating, and can play a long-term root inhibitor role; and the hydroxyl groups contained on the surface of the chitosan can be bonded with the hydroxyl groups in the asphalt, so that the root inhibitor particles have good bonding with other components such as the asphalt, thereby improving the mechanical properties and stability of the waterproof coiled material, and can still maintain high mechanical properties in a relatively harsh saline-alkali environment;

[0173] The present invention modifies calcium carbonate by firstly impregnating the calcium carbonate, wherein the impregnation liquid is polyethylene glycol and lauryl alcohol polyoxyethylene ether, which can disperse the calcium carbonate, and then treat the calcium carbonate with vinyl silane to reduce the adhesion between the calcium carbonate particles and increase the lipophilicity of the particles. The surface of the modified calcium carbonate is rich in vinyl groups, which can be connected with the carboxyl groups in asphalt, improve the compatibility between calcium carbonate and asphalt, increase the chemical affinity, and enable the calcium carbonate to be uniformly dispersed in the asphalt system, thereby enhancing the interface bonding performance with the asphalt, thereby improving the puncture resistance to a certain extent. The invention is combined with specific additives, wherein tributyl citrate is used as a plasticizer, ethylene bisstearamide is used as a lubricant, and hydroxypropyl methylcellulose has film-forming property, and enables the asphalt mixture to maintain a high viscosity, thereby enhancing the compactness and uniformity of the waterproof coiled material. The invention is combined with technical means such as specific root inhibitor particles to improve the mechanical properties and mechanical stability of the waterproof coiled material, and has good salt and alkali resistance, good waterproof performance, and excellent puncture resistance.

[0174] In the mixing step of Comparative Example 1, the root inhibitor is directly mixed with asphalt and other ingredients. On the one hand, the temperature during mixing is high, which will weaken the root blocking effect of the root inhibitor. On the other hand, the root inhibitor is directly added, and its compatibility with asphalt and other ingredients is poor, resulting in poor homogeneity and uneven dispersion of the mixture, thereby affecting the mechanical properties, puncture resistance and waterproof properties of the waterproof membrane. In addition, the root inhibitor and asphalt and other ingredients are only physically mixed, and there is no chemical bonding. The bonding force between them is weak, resulting in poor mechanical stability of the waterproof membrane, and ultimately causing a large loss of mechanical properties of the waterproof membrane in a saline-alkali environment, and a serious shortening of the service life;

[0175] In Comparative Example 2, the inorganic filler calcium carbonate is directly mixed with asphalt. Calcium carbonate itself is easy to agglomerate, and its bonding force with asphalt and other components is poor. The obtained mixture is in an agglomerated state and unevenly dispersed. Comparative Example 2 also omits the auxiliary agent component, which makes the mechanical properties and lubrication properties of the waterproof membrane low, and the adhesion between the mixture is poor, and its density and uniformity are weakened. The waterproof membrane finally obtained has poor puncture resistance, and the comprehensive properties such as mechanical properties, waterproof properties and salt-alkali resistance are all at a low level.

[0176] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0177] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a puncture-resistant waterproof coiled material, characterized in that: The preparation method comprises the steps of preparing root inhibitor particles, modified calcium carbonate, mixing and coating; The preparation of the root inhibitor particles includes preparing a root inhibitor mixed solution and a post-processing step; The steps of preparing the root inhibitor mixed solution are as follows: mixing chitosan with 0.65-0.69wt% acetic acid solution, heating to 48-52°C at a rate of 0.4-0.6°C / min, stirring at 48-52°C for 31-37min to obtain a chitosan solution; mixing trichloroacetic acid with deionized water, heating to 63-68°C at a rate of 1.0-1.4°C / min, stirring at 63-68°C for 18-23min, adding an emulsifier after stirring evenly, and performing ultrasonic oscillation treatment for 17 -22min, the ultrasonic frequency is 20-25kHz, the ultrasonic power is 113-119W, and the root inhibitor solution is obtained after the ultrasonic treatment; the chitosan solution is added to the root inhibitor solution, stirred evenly, and then homogenized, the homogenization time is 2.8-3.2min, the homogenization pressure is 6.0-6.4MPa, the homogenization times are 2 times, after the homogenization is completed, sodium tripolyphosphate is added and stirred, the stirring time is 10-15min, the stirring speed is 338-352rpm, and the stirring is completed to obtain a root inhibitor mixed solution; The mass ratio of chitosan to acetic acid solution is 1.1-1.3:100; The mass ratio of trichloroacetic acid to deionized water is 5.6-5.8 mg:100 g; The mass ratio of deionized water to emulsifier is 85-89:1.9-2.3; The emulsifier is a mixture of Tween-80 and sucrose fatty acid ester, and the mass ratio of Tween-80 to sucrose fatty acid ester is 1.6-1.8:1.1-1.3; The mass ratio of the chitosan solution, the root inhibitor solution and the sodium tripolyphosphate is 18-20:75-79:0.41-0.45; The post-treatment step is to centrifuge and wash the root inhibitor mixed liquid, and then pre-cool it, the pre-cooling time is 4.3-4.7 hours, the pre-cooling temperature is -15 to -11°C, and after the pre-cooling, vacuum freeze-drying is performed, the vacuum degree is controlled to be 60-64Pa, the cold trap temperature is -38 to -34°C, and the time is 13-15 hours. After the vacuum freeze-drying is completed, it is naturally restored to room temperature to obtain root inhibitor particles; The modified calcium carbonate comprises impregnation and modification steps; The impregnation step comprises placing calcium carbonate in a ball mill for ball milling, wherein the ball milling time is 37-43 minutes, the ball milling speed is 138-145 rpm, and the ball-to-material ratio is 4-6:

1. After the ball milling is completed, the ball-milled calcium carbonate is obtained, and the ball-milled calcium carbonate is placed in an impregnation liquid of 6-8 times the mass for static treatment, wherein the static treatment time is 17-22 minutes, the static temperature is 59-63° C., and the static pressure is 0.07-0.09 MPa. After the static treatment is completed, the calcium carbonate is naturally restored to room temperature, and the ball milling treatment is continued in the impregnation liquid, wherein the ball milling speed is 195-206 rpm, the ball milling time is 28-33 minutes, and the ball-to-material ratio is 3-5:

1. After the ball milling is completed, the calcium carbonate is dried to obtain the impregnated calcium carbonate; The impregnation liquid is composed of deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether, and the mass ratio of the deionized water, polyethylene glycol 600, polyethylene glycol 400 and lauryl alcohol polyoxyethylene ether is 120-125:1.6-1.8:1.0-1.2:1.1-1.3; The modification step is to place the impregnated calcium carbonate in an ethanol solution of 7-9 times the mass, stir evenly, heat it to 50-54°C, add the modification liquid, control the addition rate of the modification liquid to be 0.34-0.36mL / min, heat it to 67-73°C at a rate of 0.3-0.5°C / min after the addition is completed, continue stirring, the stirring time is 1.7-1.9h, the stirring speed is 197-210rpm, and after the stirring is completed, keep warm for 18-22min, and after the heat preservation is completed, filter, wash, and dry to obtain modified calcium carbonate; The modified liquid is a mixed liquid of vinyl trimethoxysilane and vinyl tri(β-methoxyethoxy)silane, and the mass ratio of the vinyl trimethoxysilane to the vinyl tri(β-methoxyethoxy)silane is 1.1-1.3:1; The mixing step is to add asphalt and softener into a reaction kettle, mix, heat up to 153-157°C, continue stirring during the heating process, the stirring speed is 370-382rpm, then heat up to 170-174°C, add SBS rubber and styrene-butadiene rubber, stir evenly, add modified calcium carbonate, root inhibitor particles, antioxidant and additives, and then use a high-speed shearing machine to shear, control the speed to 823-836rpm, and the shearing time is 92-98min. After the high-speed shearing is completed, a puncture-resistant mixture is obtained; The mass ratio of the asphalt, softener, SBS rubber, styrene-butadiene rubber, modified calcium carbonate, root inhibitor particles, antioxidant and additive is 100-104:10.2-10.4:7.3-8.1:6.4-7.0:20-24:7.4-7.6:2.0-2.4:2.1-2.5; The asphalt is a mixture of 70# asphalt and 100# asphalt, and the mass ratio of the 70# asphalt to the 100# asphalt is 1.4-1.6:1.1-1.3; The softener is a combination of paraffin oil and naphthenic oil, and the mass ratio of the paraffin oil to the naphthenic oil is 1.0-1.2:1.6-1.8; The antioxidant is a mixture of antioxidant 1098 and antioxidant 1010, and the mass ratio of the antioxidant 1098 to the antioxidant 1010 is 1.0-1.2:1.2-1.4; the auxiliary agent is a mixture of tributyl citrate, ethylene bisstearamide, and hydroxypropyl methylcellulose, and the mass ratio of the tributyl citrate, ethylene bisstearamide, and hydroxypropyl methylcellulose is 2.4-2.6:1.1-1.3:1.5-1.

9.

2. The method for preparing a puncture-resistant waterproof coiled material according to claim 1, characterized in that: In the impregnation step, the calcium carbonate is heavy calcium carbonate with a particle size of 225-235 nm.

3. The method for preparing a puncture-resistant waterproof coiled material according to claim 1, characterized in that: In the modification step, the mass concentration of the ethanol solution is 40-44%; The mass ratio of the ethanol solution to the modifying liquid is 110:1.2-1.

4.

4. The method for preparing a puncture-resistant waterproof coiled material according to claim 1, characterized in that: The coating step comprises conveying the mixture to an oil immersion tank, unfolding the tire base layer into the oil immersion tank, performing oil immersion coating, coating the puncture-resistant mixture on both sides of the tire base layer, the coating thickness of the puncture-resistant mixture is 1.6-2.0 mm, and a puncture-resistant layer is prepared, and polyethylene films are respectively covered on both sides of the puncture-resistant layer, and the thickness of the polyethylene films is 0.14-0.16 mm to form an upper covering layer and a lower covering layer, and after cooling, trimming, and rolling, a puncture-resistant waterproof coiled material is prepared; The puncture-resistant waterproof coiled material comprises, from top to bottom, an upper covering layer, an upper surface puncture-resistant layer, a base layer, a lower surface puncture-resistant layer, and a lower covering layer; The tire base layer is a polyester fiber non-woven fabric with a thickness of 0.21-0.25 mm.

5. A puncture-resistant waterproof coiled material prepared according to the preparation method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Copper plating glass fiber pad asphalt root-puncture-resistant waterproof coil

    CN109440486A

  • Novel root-puncture-resistant modified asphalt waterproof coiled material and preparation method thereof

    CN114808481A

  • Anti-root intrusion and rat and insect bite resistant subsurface drip irrigation tape

    CN107629302A

  • Modified asphalt waterproof coiled material with root penetration resistance and production method of coiled material

    CN107933035A

  • Root-resistant waterproof lignin-modified asphalt sheet and production method thereof

    CN108099320A