A silicon-based heterojunction solar cell and a method for preparing the same

By combining ZnO-based transparent conductive layer and InO-based transparent conductive layer in silicon-based heterojunction solar cells, metal electrodes in silicon-based heterojunction solar cells are solved by using ZnO-based transparent conductive layer and setting up ZnO hybrid polythiophene transition layer in metal electrodes. The problem of large contact resistance with transparent conductive oxide layer improves battery performance and reduces the use of InO, achieving good conductivity and anti-reflection effects.

CN118472084BActive Publication Date: 2024-11-26ZHEJIANG WINHITECH NEW ENERGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410939842.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-26
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

During the annealing process of existing silicon-based heterojunction solar cells, the contact resistance between the metal electrode and the transparent conductive oxide layer is large, resulting in poor electrical performance, and the use of the InO-based transparent conductive layer has environmental and health hazards.

Method used

The transition layer containing the electrode conductive metal and ZnO hybrid polythiophene is arranged in the metal electrode by combining the ZnO hybrid polythiophene with the electrode layer. The metal electrode and ZnO hybrid polythiophene are combined with the electrode layer are reduced. The contact resistance of the base transparent conductive layer is formed by a conductive path through polythiophene to reduce the resistance.

Benefits of technology

It effectively reduces the contact resistance between the metal electrode and the ZnO-based transparent conductive layer, improves the photoelectric conversion efficiency of the solar cell, and reduces the use of InO, ensuring the conductive performance and anti-reflection effect of the TCO layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118472084B_ABST
    Figure CN118472084B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solar cells, and discloses a silicon-based heterojunction solar cell and a preparation method thereof. The silicon-based heterojunction solar cell comprises a heterojunction silicon substrate; the front and back sides of the heterojunction silicon substrate are sequentially provided with an InO-based transparent conductive layer, a ZnO-based transparent conductive layer and a metal electrode; the metal electrode comprises an electrode layer and a transition layer provided between the electrode layer and the ZnO-based transparent conductive layer; the material of the electrode layer comprises an electrode conductive metal, and the material of the transition layer comprises an electrode conductive metal and a ZnO hybrid polythiophene, wherein the ZnO hybrid polythiophene is composed of a polythiophene with a hydroxyl group on the side chain and ZnO bonded to the hydroxyl group. The silicon-based heterojunction solar cell of the present invention can reduce the contact resistance between the metal electrode and the ZnO-based transparent conductive layer by providing a transition layer containing an electrode conductive metal and ZnO hybrid polythiophene in the metal electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a silicon-based heterojunction solar cell and a preparation method thereof. Background Art

[0002] The basic structure of silicon-based heterojunction (SHJ) solar cells includes a heterojunction silicon substrate, a transparent conductive oxide (TCO) layer and a metal electrode, which has the advantages of high photoelectric conversion efficiency and low temperature coefficient. The preparation method of SHJ solar cells is to deposit a TCO layer on a heterojunction silicon substrate composed of crystalline silicon and amorphous silicon, and then print a metal electrode for conducting current on the TCO layer. In the above process, after printing the electrode metal paste on the TCO layer, the annealing temperature usually cannot exceed 250°C. When the temperature is too high, it will have an adverse effect on the performance of the SHJ cell. Therefore, sintering between the TCO and the electrode metal material cannot occur during annealing, which will cause more defects at the interface between the two, and the contact resistance is large, which will affect the electrical performance of the SHJ cell.

[0003] Patent CN202210104124.9 discloses a conductive silver paste composition with low contact resistivity with a TCO transparent conductive film layer, in which ultrafine silver oxide that can be thermally decomposed is added to the conductive silver paste, which decomposes into elemental silver during the annealing (thermal curing) process, and can reduce the contact resistivity between the metal electrode and the TCO layer. However, the solution of this patent has the following problems: thermal decomposition of silver oxide will produce oxygen, which is easy to produce holes in the interface between the electrode and the TCO layer, which limits the reduction of the contact resistance between the electrode and the TCO layer. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a silicon-based heterojunction solar cell. The silicon-based heterojunction solar cell can reduce the contact resistance between the metal electrode and the ZnO-based transparent conductive layer by providing a transition layer containing an electrode conductive metal and ZnO hybrid polythiophene in the metal electrode.

[0005] The specific technical scheme of the present invention is:

[0006] In a first aspect, the present invention provides a silicon-based heterojunction solar cell, comprising a heterojunction silicon substrate; the front and back sides of the heterojunction silicon substrate are sequentially provided with an InO-based transparent conductive layer, a ZnO-based transparent conductive layer and a metal electrode; the metal electrode comprises an electrode layer and a transition layer provided between the electrode layer and the ZnO-based transparent conductive layer; the material of the electrode layer comprises an electrode conductive metal, the material of the transition layer comprises an electrode conductive metal and a ZnO hybrid polythiophene, and the ZnO hybrid polythiophene is composed of a polythiophene having a hydroxyl group on a side chain and ZnO bonded to the hydroxyl group.

[0007] InO is a commonly used TCO material in solar cells, but In is a precious metal material with a scarce source, and its production process is prone to produce toxic fumes, which are harmful to the environment and human body. The present invention uses an InO-based transparent conductive layer and a ZnO-based transparent conductive layer as a TCO layer in a silicon-based heterojunction solar cell, which can reduce the use of InO while ensuring the anti-reflection effect and conductive performance of the TCO layer.

[0008] The present invention provides a transition layer in the metal electrode, which contains ZnO and an electrode conductive metal, and ZnO is bonded to the side chain hydroxyl group of polythiophene, which can prevent ZnO from agglomerating, so that it is dispersed in the transition layer with a finer particle size and can be filled in the gap at the interface between the electrode conductive metal and the ZnO-based transparent conductive layer. In the above manner, the transition layer can be well combined with the ZnO-based transparent conductive layer and the electrode layer to achieve a lower contact resistance. In addition, since ZnO is bonded to polythiophene, the polythiophene can be used to form a conductive path to reduce the resistance of the transition layer.

[0009] Preferably, the polythiophene with hydroxyl groups on the side chains is a copolymer of 3-hexylthiophene and thiophene-3-ethanol, and the mass ratio of 3-hexylthiophene to thiophene-3-ethanol is 1:0.07-0.15.

[0010] By copolymerizing 3-hexylthiophene and thiophene-3-ethanol, hydroxyl groups can be introduced into the side chains of the obtained polythiophene molecular chains by utilizing thiophene-3-ethanol.

[0011] Preferably, in the transition layer, the mass ratio between the electrode conductive metal and the ZnO hybrid polythiophene is 1:0.05-0.08.

[0012] Preferably, the thickness of the InO-based transparent conductive layer is 20-50 nm, wherein the content of InO is not less than 90%; the thickness of the ZnO-based transparent conductive layer is 20-60 nm, wherein the content of ZnO is not less than 90%.

[0013] Preferably, on the front side of the heterojunction silicon substrate, a Si3N4 layer is provided outside the ZnO-based transparent conductive layer, and the metal electrode penetrates the Si3N4 layer.

[0014] Preferably, the thickness of the Si3N4 layer is 10-30 nm, and the thickness of the metal electrode is 5-10 μm.

[0015] Preferably, the heterojunction silicon substrate comprises an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer, a double-textured p-type single crystal silicon substrate and an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer stacked in sequence.

[0016] Preferably, the thicknesses of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer and the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer are 15-35 nm and 10-30 nm, respectively.

[0017] Preferably, the thickness of the transition layer is 1-2 μm.

[0018] In a second aspect, the present invention provides a method for preparing the silicon-based heterojunction solar cell, comprising the following steps:

[0019] (1) An InO-based transparent conductive layer and a ZnO-based transparent conductive layer are sequentially deposited on the front and back sides of the heterojunction silicon substrate;

[0020] (2) Adding ZnO hybrid polythiophene slurry to electrode metal slurry, printing transition layers on the surfaces of the ZnO-based transparent conductive layers on the front and back sides; and then using electrode metal slurry to print electrode layers on the surfaces of the transition layers to form metal electrodes.

[0021] Preferably, after step (2), Si3N4 is deposited on the surface of the ZnO-based transparent conductive layer on the front side to form a Si3N4 layer having a thickness less than that of the metal electrode.

[0022] In the prior art, the order of first depositing the Si3N4 layer and then printing the metal electrode is adopted. When this preparation order is adopted in the present invention, the formed metal electrode is difficult to form a good contact with the ZnO-based transparent conductive layer. It is necessary to open the Si3N4 layer before printing the metal electrode, which is relatively complicated. To this end, the present invention first prepares the metal electrode on the ZnO-based transparent conductive layer, and then deposits the Si3N4 layer with a thickness less than the metal electrode. It is not necessary to open the Si3N4 layer to avoid the Si3N4 layer affecting the contact between the metal electrode and the ZnO-based transparent conductive layer. At the same time, it can ensure that the three-layer composite film composed of the InO-based transparent conductive layer, the ZnO-based transparent conductive layer and the Si3N4 layer has a good anti-reflection effect.

[0023] Preferably, the preparation steps of the ZnO hybrid polythiophene include:

[0024] (A) 3-hexylthiophene and thiophene-3-ethanol are copolymerized to prepare polythiophene with hydroxyl groups on the side chains;

[0025] (B) Using alcohol zinc salt and polythiophene with hydroxyl groups on the side chain as raw materials, ZnO is formed by reaction on the hydroxyl groups in the polythiophene with hydroxyl groups on the side chain to obtain ZnO hybrid polythiophene.

[0026] In step (B), the alcohol zinc salt can be converted into ZnO through hydrolysis reaction and condensation reaction, and the generated ZnO is chelated on the side chain hydroxyl group of polythiophene. In this way, ZnO with finer particle size can be obtained and its agglomeration can be prevented.

[0027] Preferably, the specific process of step (A) comprises: dissolving 3-hexylthiophene and thiophene-3-ethanol in an organic solvent to prepare a thiophene solution; dissolving a catalyst in an organic solvent to prepare a catalyst solution; adding the thiophene solution dropwise to the catalyst solution, reacting at 20-30° C. for 20-25 h, separating the product, and preparing a polythiophene with a hydroxyl group on the side chain.

[0028] Preferably, in step (A), the catalyst is ferric chloride; and the ratio of the total mass of 3-hexylthiophene and thiophene-3-ethanol to the mass of ferric chloride is 1:2.5-4.0.

[0029] Preferably, the specific process of step (B) comprises: dissolving polythiophene having a hydroxyl group on the side chain in a non-protonic solvent to prepare a polymer solution; dissolving an alcohol zinc salt in an aprotic solvent to prepare an alcohol zinc salt solution; adding water to the polymer solution, adding the alcohol zinc salt solution under stirring, reacting at 30-40° C. for 1-2 h, and then reacting at 130-140° C. for 1-2 h.

[0030] Preferably, in step (B), the alkoxide zinc salt is zinc methoxide and / or zinc isopropoxide.

[0031] Preferably, in step (B), the mass ratio of the polythiophene having a hydroxyl group on the side chain to the zinc salt of alcohol is 1:0.3-0.5.

[0032] Preferably, in step (B), the volume ratio of the polymer solution to water is 1:0.001-0.002.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] (1) The present invention uses an InO-based transparent conductive layer and a ZnO-based transparent conductive layer as a composite TCO layer, which can reduce the use of InO while ensuring the anti-reflection effect and conductive performance of the TCO layer.

[0035] (2) The present invention can reduce the contact resistance between the metal electrode and the ZnO-based transparent conductive layer by providing a transition layer containing an electrode conductive metal and ZnO hybrid polythiophene in the metal electrode.

[0036] (3) In the process of preparing silicon-based heterojunction solar cells, the present invention first prepares a metal electrode on the front ZnO-based transparent conductive layer, and then deposits a Si3N4 layer. This is beneficial for better contact between the metal electrode and the ZnO-based transparent conductive layer, reducing contact resistance, and at the same time, it can also make the three-layer composite film composed of the InO-based transparent conductive layer, the ZnO-based transparent conductive layer and the Si3N4 layer have a good anti-reflection effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A schematic diagram of the structure of a silicon-based heterojunction solar cell of the present invention.

[0038] The reference numerals are: heterojunction silicon substrate 1, double-textured p-type single crystal silicon substrate 101, intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer 102, intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer 103, InO-based transparent conductive layer 2, ZnO-based transparent conductive layer 3, metal electrode 4, electrode layer 401, transition layer 402, Si3N4 layer 5. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the embodiments.

[0040] A silicon-based heterojunction solar cell comprises a heterojunction silicon substrate; the front and back sides of the heterojunction silicon substrate are sequentially provided with an InO-based transparent conductive layer, a ZnO-based transparent conductive layer and a metal electrode; the metal electrode comprises an electrode layer and a transition layer provided between the electrode layer and the ZnO-based transparent conductive layer; the material of the electrode layer comprises an electrode conductive metal, the material of the transition layer comprises an electrode conductive metal and a ZnO hybrid polythiophene, and the ZnO hybrid polythiophene comprises a polythiophene with a hydroxyl group on the side chain and ZnO bonded to the hydroxyl group.

[0041] As a specific implementation, the polythiophene with hydroxyl groups on the side chain is a copolymer of 3-hexylthiophene and thiophene-3-ethanol, and the mass ratio of 3-hexylthiophene to thiophene-3-ethanol is 1:0.07-0.15.

[0042] As a specific implementation, in the transition layer, the mass ratio between the electrode conductive metal and the ZnO hybrid polythiophene is 1:0.05-0.08.

[0043] As a specific implementation, the thickness of the InO-based transparent conductive layer is 20-50 nm, wherein the content of InO is not less than 90%; the thickness of the ZnO-based transparent conductive layer is 20-60 nm, wherein the content of ZnO is not less than 90%.

[0044] As a specific implementation, on the front side of the heterojunction silicon substrate, a Si3N4 layer is provided outside the ZnO-based transparent conductive layer, and the metal electrode penetrates the Si3N4 layer; the thickness of the Si3N4 layer is 10~30 nm, the thickness of the metal electrode is 5~10 μm, and the thickness of the transition layer is 1~2 μm.

[0045] As a specific implementation, the heterojunction silicon substrate includes an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer, a double-textured p-type single crystal silicon substrate and an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer stacked in sequence; the thicknesses of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer and the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer are 15~35 nm and 10~30 nm, respectively.

[0046] A method for preparing the silicon-based heterojunction solar cell comprises the following steps:

[0047] (1) An InO-based transparent conductive layer and a ZnO-based transparent conductive layer are sequentially deposited on the front and back sides of the heterojunction silicon substrate;

[0048] (2) Adding ZnO hybrid polythiophene slurry to electrode metal slurry, printing transition layers on the surfaces of the ZnO-based transparent conductive layers on the front and back sides; and then using electrode metal slurry to print electrode layers on the surfaces of the transition layers to form metal electrodes.

[0049] As a specific implementation, after step (2), Si3N4 is deposited on the surface of the ZnO-based transparent conductive layer on the front side to form a Si3N4 layer with a thickness less than that of the metal electrode.

[0050] As a specific implementation, the preparation steps of the ZnO hybrid polythiophene include:

[0051] (A) 3-hexylthiophene and thiophene-3-ethanol are copolymerized to prepare polythiophene with hydroxyl groups on the side chains;

[0052] (B) Using alcohol zinc salt and polythiophene with hydroxyl groups on the side chain as raw materials, ZnO is formed by reaction on the hydroxyl groups in the polythiophene with hydroxyl groups on the side chain to obtain ZnO hybrid polythiophene.

[0053] As a specific implementation method, the specific process of step (A) includes: dissolving 3-hexylthiophene and thiophene-3-ethanol in an organic solvent to prepare a thiophene solution, wherein the total concentration of 3-hexylthiophene and thiophene-3-ethanol is 0.02-0.04 g / mL; dissolving a catalyst in an organic solvent to prepare a 0.04-0.07 g / mL catalyst solution; adding the thiophene solution dropwise to the catalyst solution, reacting at 20-30° C. for 20-25 h, separating the product, and preparing a polythiophene with a hydroxyl group on the side chain.

[0054] As a specific implementation, in step (B), the alkoxide zinc salt is zinc methoxide and / or zinc isopropoxide; and the mass ratio of the polythiophene having a hydroxyl group on the side chain to the alkoxide zinc salt is 1:0.3-0.5.

[0055] As a specific implementation method, the specific process of step (B) includes: dissolving polythiophene with hydroxyl groups on the side chain in a non-protonic solvent to prepare a 0.06-0.09 g / mL polymer solution; dissolving an alcohol zinc salt in an aprotic solvent to prepare a 0.04-0.08 g / mL alcohol zinc salt solution; adding water to the polymer solution, wherein the volume ratio of the polymer solution to water is 1:0.001-0.002, and then adding the alcohol zinc salt solution under stirring, reacting at 30-40°C for 1-2 h, and then reacting at 130-140°C for 1-2 h.

[0056] In step (2), the electrode metal slurry may be a conventional electrode metal slurry. An optional specific formula is provided below, comprising the following components in parts by weight: 80-85 parts of silver powder, 4-7 parts of epoxy resin, 0.5-0.8 parts of curing agent, 3-8 parts of diluent, 0-1 parts of dispersant, and 0-1 parts of adhesion promoter.

[0057] The present invention is described below by specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention, and the attached claims and any equivalents thereof are the protection scope of the present invention.

[0058] Unless otherwise defined, all technical terms and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the field to which the present disclosure belongs. Unless otherwise specified, the raw materials and equipment used in the present invention are conventional raw materials and equipment in the field and can be obtained from conventional commercial channels; unless otherwise specified, the methods used in the present invention are conventional methods in the field.

[0059] In the following examples and comparative examples, the abbreviations involved have the following meanings:

[0060] DMSO: dimethyl sulfoxide;

[0061] DMF: N,N-dimethylformamide;

[0062] PT-OH: polythiophene with hydroxyl groups on the side chain;

[0063] Eff: Photoelectric conversion efficiency.

[0064] Example 1

[0065] The ZnO hybrid polythiophene slurry used in this example was prepared by the following steps:

[0066] (A) 3-hexylthiophene and thiophene-3-ethanol were dissolved in DMSO to prepare a thiophene solution with a total concentration of 0.03 g / mL (total concentration of 3-hexylthiophene and thiophene-3-ethanol). Under nitrogen protection, anhydrous FeCl3 was dissolved in DMSO to prepare a 0.05 g / mL FeCl3 solution, to which the thiophene solution was added dropwise and stirred at room temperature (about 26°C) for 24 h. After the reaction was completed, methanol was added to precipitate the product, which was filtered and dried to obtain PT-OH. In the above process, the mass ratio between 3-hexylthiophene, thiophene-3-ethanol and anhydrous FeCl3 was 1:0.1:3.2.

[0067] (B) Dissolve zinc isopropoxide in DMF to prepare a 0.05 g / mL zinc isopropoxide solution. Dissolve PT-OH in DMF to prepare a 0.08 g / mL PT-OH solution, add water thereto, add the zinc isopropoxide solution under stirring, and then stir and react at 40°C for 1 h, then heat to 130°C and continue stirring and reacting for 2 h. After the reaction is completed, the obtained mixed solution is concentrated under reduced pressure to 1 / 5 of the original volume to obtain a ZnO hybrid polythiophene slurry. In the above process, the mass ratio of PT-OH to zinc isopropoxide is 1:0.4, and the volume ratio of PT-OH solution to water is 1:0.001.

[0068] The electrode metal paste used in this embodiment has the following formula (each component is measured in parts by weight): 85 parts of silver powder, 5 parts of epoxy resin, 0.6 parts of phthalic anhydride, 5 parts of butyl acetate, 2 parts of benzyl glycidyl ether, 0.1 parts of dispersant BYK-111, and 0.1 parts of adhesion promoter BYK-4512.

[0069] The structure of the silicon-based heterojunction solar cell in this embodiment is as follows Figure 1 As shown, the specific details are as follows: it includes a heterojunction silicon substrate 1; the heterojunction silicon substrate 1 is composed of an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer 103, a double-textured p-type single crystal silicon substrate 101 and an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer 102 stacked in sequence; an InO-based transparent conductive layer 2, a ZnO-based transparent conductive layer 3 and a metal electrode 4 are sequentially provided on the front side (i.e., the side where the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer 102 is located) and the back side (i.e., the side where the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer 103 is located) of the heterojunction silicon substrate 1; the metal electrode 4 is composed of an electrode layer 401 and a transition layer 402, and the transition layer 402 is provided between the electrode layer 401 and the ZnO-based transparent conductive layer 3; on the front side of the heterojunction silicon substrate 1, a Si3N4 layer 5 is provided outside the ZnO-based transparent conductive layer 3, and the metal electrode 4 on the front side penetrates the Si3N4 layer 5.

[0070] The silicon-based heterojunction solar cell of this embodiment is prepared by the following steps:

[0071] (1) By plasma chemical vapor deposition, an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer with a thickness of 20 nm and an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer with a thickness of 25 nm were deposited on the front and back sides of a double-textured p-type single crystal silicon substrate, respectively.

[0072] (2) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 30 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0073] (3) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 35 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0074] (4) The ZnO hybrid polythiophene slurry prepared in this example is mixed with the electrode metal slurry so that the mass ratio of ZnO hybrid polythiophene to silver powder is 0.08:1 to prepare a transition layer slurry.

[0075] (5) The transition layer slurry is printed on the outer surface of the ZnO-based transparent conductive layer on the front and back sides by screen printing, and annealed at 200°C for 5 min to form a transition layer. Then, the electrode metal slurry is printed on the outer surface of the transition layer by screen printing, and annealed at 200°C for 10 min to form an electrode layer, thereby forming a metal electrode consisting of a transition layer and an electrode layer on the outer surface of the ZnO-based transparent conductive layer, wherein the thickness of the metal electrode is 9 μm, of which the thickness of the transition layer is 1 μm.

[0076] (6) A Si3N4 layer with a thickness of 20 nm is deposited on the outer surface of the ZnO-based transparent conductive layer on the front side by chemical vapor deposition.

[0077] It was measured that in the silicon-based heterojunction solar cell prepared in this embodiment, the contact resistivity between the metal electrode and the ZnO-based transparent conductive layer was 1.07 mΩ / cm 2 , the battery Eff is 23.77%.

[0078] Example 2

[0079] The ZnO hybrid polythiophene slurry used in this example was prepared by the following steps:

[0080] (A) 3-hexylthiophene and thiophene-3-ethanol were dissolved in DMSO to prepare a thiophene solution with a total concentration of 0.04 g / mL (total concentration of 3-hexylthiophene and thiophene-3-ethanol). Under nitrogen protection, anhydrous FeCl3 was dissolved in DMSO to prepare a 0.04 g / mL FeCl3 solution, to which the thiophene solution was added dropwise and stirred at room temperature (about 26°C) for 20 h. After the reaction was completed, methanol was added to precipitate the product, which was filtered and dried to obtain PT-OH. In the above process, the mass ratio between 3-hexylthiophene, thiophene-3-ethanol and anhydrous FeCl3 was 1:0.15:4.5.

[0081] (B) Dissolve zinc isopropoxide in DMF to prepare a 0.04 g / mL zinc isopropoxide solution. Dissolve PT-OH in DMF to prepare a 0.09 g / mL PT-OH solution, add water thereto, add the zinc isopropoxide solution under stirring, and then stir and react at 30°C for 2 h, then heat to 140°C and continue stirring and reacting for 1 h. After the reaction is completed, the obtained mixed solution is concentrated under reduced pressure to 1 / 5 of the original volume to obtain a ZnO hybrid polythiophene slurry. In the above process, the mass ratio of PT-OH to zinc isopropoxide is 1:0.3, and the volume ratio of PT-OH solution to water is 1:0.002.

[0082] The electrode metal slurry formula used in this embodiment is the same as that in Example 1.

[0083] The silicon-based heterojunction solar cell structure of this embodiment is the same as that of Embodiment 1, and is prepared by the following steps:

[0084] (1) By plasma chemical vapor deposition, an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer with a thickness of 10 nm and an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer with a thickness of 15 nm were deposited on the front and back sides of a double-textured p-type single crystal silicon substrate, respectively.

[0085] (2) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 20 nm and a ZnO-based transparent conductive layer with a thickness of 50 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0086] (3) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 20 nm and a ZnO-based transparent conductive layer with a thickness of 60 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0087] (4) The ZnO hybrid polythiophene slurry prepared in this example is mixed with the electrode metal slurry so that the mass ratio of ZnO hybrid polythiophene to silver powder is 0.08:1 to prepare a transition layer slurry.

[0088] (5) The transition layer slurry is printed on the outer surface of the ZnO-based transparent conductive layer on the front and back sides by screen printing, and annealed at 200°C for 5 min to form a transition layer. Then, the electrode metal slurry is printed on the outer surface of the transition layer by screen printing, and annealed at 200°C for 10 min to form an electrode layer, thereby forming a metal electrode consisting of a transition layer and an electrode layer on the outer surface of the ZnO-based transparent conductive layer, wherein the thickness of the metal electrode is 9 μm, of which the thickness of the transition layer is 1 μm.

[0089] (6) A Si3N4 layer with a thickness of 30 nm is deposited on the outer surface of the ZnO-based transparent conductive layer on the front side by chemical vapor deposition. After cutting, a silicon-based heterojunction solar cell is obtained.

[0090] It was measured that in the silicon-based heterojunction solar cell prepared in this embodiment, the contact resistivity between the metal electrode and the ZnO-based transparent conductive layer was 1.16 mΩ / cm 2 , the battery Eff is 23.24%.

[0091] Example 3

[0092] The ZnO hybrid polythiophene slurry used in this example was prepared by the following steps:

[0093] (A) 3-hexylthiophene and thiophene-3-ethanol were dissolved in DMSO to prepare a thiophene solution of 0.02 g / mL (total concentration of 3-hexylthiophene and thiophene-3-ethanol). Under nitrogen protection, anhydrous FeCl3 was dissolved in DMSO to prepare a 0.07 g / mL FeCl3 solution, to which the thiophene solution was added dropwise, and the reaction was stirred at room temperature (about 26°C) for 25 h. After the reaction was completed, methanol was added to precipitate the product, which was filtered and dried to obtain PT-OH. In the above process, the mass ratio between 3-hexylthiophene, thiophene-3-ethanol and anhydrous FeCl3 was 1:0.07:0.18.

[0094] (B) Dissolve zinc isopropoxide in DMF to prepare a 0.08 g / mL zinc isopropoxide solution. Dissolve PT-OH in DMF to prepare a 0.06 g / mL PT-OH solution, add water thereto, add the zinc isopropoxide solution under stirring, and then stir and react at 35°C for 1.5 h, then heat to 135°C and continue stirring and reacting for 1.5 h. After the reaction is completed, the obtained mixed solution is concentrated under reduced pressure to 1 / 5 of the original volume to obtain a ZnO hybrid polythiophene slurry. In the above process, the mass ratio of PT-OH to zinc isopropoxide is 1:0.5, and the volume ratio of PT-OH solution to water is 1:0.001.

[0095] The electrode metal slurry formula used in this embodiment is the same as that in Example 1.

[0096] The silicon-based heterojunction solar cell structure of this embodiment is the same as that of Embodiment 1, and is prepared by the following steps:

[0097] (1) By plasma chemical vapor deposition, an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer with a thickness of 30 nm and an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer with a thickness of 35 nm were deposited on the front and back sides of a double-textured p-type single crystal silicon substrate, respectively.

[0098] (2) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 50 nm and a ZnO-based transparent conductive layer with a thickness of 30 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0099] (3) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 50 nm and a ZnO-based transparent conductive layer with a thickness of 20 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0100] (4) The ZnO hybrid polythiophene slurry prepared in this example is mixed with the electrode metal slurry so that the mass ratio of ZnO hybrid polythiophene to silver powder is 0.05:1 to prepare a transition layer slurry.

[0101] (5) Using screen printing, a transition layer slurry is printed on the outer surface of the ZnO-based transparent conductive layer on the front and back sides, and annealed at 200-250°C for 5-10 min to form a transition layer. Then, an electrode metal slurry is printed on the outer surface of the transition layer by screen printing, and annealed at 200-250°C for 5-10 min to form an electrode layer, thereby forming a metal electrode consisting of a transition layer and an electrode layer on the outer surface of the ZnO-based transparent conductive layer, wherein the thickness of the metal electrode is 9 μm, of which the thickness of the transition layer is 1 μm.

[0102] (6) A Si3N4 layer with a thickness of 10 nm is deposited on the outer surface of the ZnO-based transparent conductive layer on the front side by chemical vapor deposition. After cutting, a silicon-based heterojunction solar cell is obtained.

[0103] It was measured that in the silicon-based heterojunction solar cell prepared in this embodiment, the contact resistivity between the metal electrode and the ZnO-based transparent conductive layer was 1.20 mΩ / cm 2 , the battery Eff is 23.83%.

[0104] Comparative Example 1

[0105] The difference between this comparative example and Example 1 is that the metal electrode is only composed of an electrode layer without a transition layer. The rest of the raw materials and steps are the same as those of Example 1. Specifically:

[0106] The electrode metal slurry formula used in this comparative example is the same as that in Example 1.

[0107] The silicon-based heterojunction solar cell of this comparative example is prepared by the following steps:

[0108] (1) By plasma chemical vapor deposition, an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer with a thickness of 20 nm and an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer with a thickness of 25 nm were deposited on the front and back sides of a double-textured p-type single crystal silicon substrate, respectively.

[0109] (2) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 30 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0110] (3) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 35 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0111] (4) The electrode metal paste is printed onto the outer surface of the transition layer by screen printing and annealed at 200°C for 10 min to form a metal electrode with a thickness of 10 μm.

[0112] (5) A Si3N4 layer with a thickness of 20 nm is deposited on the outer surface of the ZnO-based transparent conductive layer on the front side by chemical vapor deposition. After cutting, a silicon-based heterojunction solar cell is obtained.

[0113] It was measured that in the silicon-based heterojunction solar cell prepared in this comparative example, the contact resistivity between the metal electrode and the ZnO-based transparent conductive layer was 3.84 mΩ / cm 2 , the battery Eff is 22.57%. The contact resistance of this comparative example is significantly greater than that of Example 1, and the battery Eff is less than that of Example 1, because: Example 1 sets a transition layer containing ZnO hybrid polythiophene and silver powder in the metal electrode, and the transition layer can be well combined with the ZnO-based transparent conductive layer and the electrode layer, so that the contact resistance between the metal electrode and the ZnO-based transparent conductive layer can be effectively reduced, and the photoelectric conversion efficiency of the battery can be improved.

[0114] Comparative Example 2

[0115] The difference between this comparative example and Example 1 is that zinc oxide is not bonded to the hydroxyl group in polythiophene, but zinc oxide and polythiophene are dispersed and added to the electrode metal slurry. The rest of the raw materials and steps are the same as Example 1. Specifically:

[0116] The ZnO / polythiophene mixed slurry used in this comparative example was prepared by the following steps:

[0117] (A) 3-hexylthiophene and thiophene-3-ethanol were dissolved in DMSO to prepare a thiophene solution with a total concentration of 0.03 g / mL (total concentration of 3-hexylthiophene and thiophene-3-ethanol). Under nitrogen protection, anhydrous FeCl3 was dissolved in DMSO to prepare a 0.05 g / mL FeCl3 solution, to which the thiophene solution was added dropwise and stirred at room temperature (about 26°C) for 24 h. After the reaction was completed, methanol was added to precipitate the product, which was filtered and dried to obtain PT-OH. In the above process, the mass ratio between 3-hexylthiophene, thiophene-3-ethanol and anhydrous FeCl3 was 1:0.1:3.2.

[0118] (B) PT-OH, nano ZnO powder and DMF were mixed in a mass volume ratio of 1 g:0.26 g:3.5 mL to prepare a ZnO / polythiophene mixed slurry.

[0119] The electrode metal slurry formula used in this comparative example is the same as that in Example 1.

[0120] (1) By plasma chemical vapor deposition, an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer with a thickness of 20 nm and an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer with a thickness of 25 nm were deposited on the front and back sides of a double-textured p-type single crystal silicon substrate, respectively.

[0121] (2) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 30 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0122] (3) By magnetron sputtering, an InO-based transparent conductive layer with a thickness of 35 nm and a ZnO-based transparent conductive layer with a thickness of 40 nm are sequentially deposited on the outer surface of the intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer. The InO-based transparent conductive layer is indium tin oxide with an indium oxide content of 90%; the ZnO-based transparent conductive layer is pure ZnO.

[0123] (4) The ZnO / polythiophene mixed slurry prepared in this comparative example was mixed with the electrode metal slurry so that the mass ratio of the total mass of PT-OH and ZnO to the mass of the silver powder was 0.08:1 to prepare a transition layer slurry.

[0124] (5) The transition layer slurry is printed on the outer surface of the ZnO-based transparent conductive layer on the front and back sides by screen printing, and annealed at 200°C for 5 min to form a transition layer. Then, the electrode metal slurry is printed on the outer surface of the transition layer by screen printing, and annealed at 200°C for 10 min to form an electrode layer, thereby forming a metal electrode consisting of a transition layer and an electrode layer on the outer surface of the ZnO-based transparent conductive layer, wherein the thickness of the metal electrode is 9 μm, of which the thickness of the transition layer is 1 μm.

[0125] (6) A Si3N4 layer with a thickness of 20 nm is deposited on the outer surface of the ZnO-based transparent conductive layer on the front side by chemical vapor deposition. After cutting, a silicon-based heterojunction solar cell is obtained.

[0126] It was measured that in the silicon-based heterojunction solar cell prepared in this comparative example, the contact resistivity between the metal electrode and the ZnO-based transparent conductive layer was 3.23 mΩ / cm 2, the battery Eff is 22.85%. The contact resistance of this comparative example is significantly greater than that of Example 1, and the battery Eff is less than that of Example 1, because: in Example 1, the ZnO converted from the alcohol zinc salt is bonded to the side chain hydroxyl group of the polythiophene, which can prevent ZnO from agglomerating, so that it is dispersed in the transition layer with a finer particle size, and can fill the gap at the interface between the electrode conductive metal and the ZnO-based transparent conductive layer, thereby reducing the contact resistance between the metal electrode and the ZnO-based transparent conductive layer to a greater extent, and improving the battery Eff.

[0127] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A silicon-based heterojunction solar cell, characterized in that: The invention comprises a heterojunction silicon substrate; the front and back sides of the heterojunction silicon substrate are sequentially provided with an InO-based transparent conductive layer, a ZnO-based transparent conductive layer and a metal electrode; the metal electrode comprises an electrode layer and a transition layer provided between the electrode layer and the ZnO-based transparent conductive layer; the material of the electrode layer comprises an electrode conductive metal; the transition layer is formed by adding a ZnO hybrid polythiophene slurry into an electrode metal slurry; the ZnO hybrid polythiophene is obtained by reacting a hydroxyl group in the polythiophene with a hydroxyl group on an alcohol zinc salt and a side chain of the polythiophene with a hydroxyl group as raw materials to form ZnO.

2. The silicon-based heterojunction solar cell according to claim 1, characterized in that: The polythiophene with hydroxyl groups on the side chain is a copolymer of 3-hexylthiophene and thiophene-3-ethanol, and the mass ratio of 3-hexylthiophene to thiophene-3-ethanol is 1:0.07-0.

15.

3. The silicon-based heterojunction solar cell according to claim 1, characterized in that: In the transition layer, the mass ratio between the electrode conductive metal and the ZnO hybrid polythiophene is 1:0.05-0.

08.

4. The silicon-based heterojunction solar cell according to claim 1, characterized in that: The thickness of the InO-based transparent conductive layer is 20-50 nm, wherein the content of InO is not less than 90%; the thickness of the ZnO-based transparent conductive layer is 20-60 nm, wherein the content of ZnO is not less than 90%.

5. The silicon-based heterojunction solar cell according to claim 1, characterized in that: On the front side of the heterojunction silicon substrate, a Si3N4 layer is provided outside the ZnO-based transparent conductive layer, and a metal electrode penetrates the Si3N4 layer.

6. The silicon-based heterojunction solar cell according to claim 5, characterized in that: The thickness of the Si3N4 layer is 10-30 nm, and the thickness of the metal electrode is 5-10 μm.

7. The silicon-based heterojunction solar cell according to claim 1, characterized in that: The heterojunction silicon substrate comprises an intrinsic amorphous silicon / p-type nanocrystalline silicon composite layer, a double-textured p-type single crystal silicon substrate and an intrinsic amorphous silicon / n-type nanocrystalline silicon composite layer which are stacked in sequence.

8. A method for preparing a silicon-based heterojunction solar cell according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) An InO-based transparent conductive layer and a ZnO-based transparent conductive layer are sequentially deposited on the front and back sides of the heterojunction silicon substrate; (2) adding ZnO hybrid polythiophene slurry to electrode metal slurry and printing transition layers on the surface of the ZnO-based transparent conductive layer on the front and back sides; Then, an electrode layer is printed on the surface of the transition layer using electrode metal paste to form a metal electrode.

9. The preparation method according to claim 8, characterized in that: After step (2), Si3N4 is deposited on the surface of the ZnO-based transparent conductive layer on the front side to form a Si3N4 layer with a thickness less than that of the metal electrode.

10. The preparation method according to claim 8, characterized in that: The preparation steps of the ZnO hybrid polythiophene include: (A) 3-hexylthiophene and thiophene-3-ethanol are copolymerized to prepare polythiophene with hydroxyl groups on the side chains; (B) Using alcohol zinc salt and polythiophene with hydroxyl groups on the side chain as raw materials, ZnO is formed by reaction on the hydroxyl groups in the polythiophene with hydroxyl groups on the side chain to obtain ZnO hybrid polythiophene.

Citation Information

Patent Citations

  • Conductive silver adhesive composition with low contact resistivity with TCO transparent conductive film layer

    CN114121339A

  • Paste for forming of an electrode of a solar cell

    CN102473741A

  • Conductive transparent high polymer material and preparation method thereof

    CN108485263A

  • Heterojunction solar cell and preparation method and application thereof

    CN114597270A

  • Solar cell

    CN116033764A