A kind of low oxygen content polydimethylsilane and preparation method thereof

By using high-temperature evaporation and cleaning solvent separation technology in the preparation of polydimethylsilane, the oxygen content and alkali metal ions are reduced, the problems of high oxygen content and impurity content in the prior art are solved, and the silicon carbide ceramics are improved Performance and simplify the cleaning process.

CN118480180BActive Publication Date: 2024-11-15TIANJIN LIGHT FUTURE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410913709.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-15
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

In the existing polydimethylsilane preparation methods, the oxygen content and impurity content are high, resulting in poor high-temperature anti-oxidation and mechanical properties of silicon carbide ceramics, and the cleaning process is complicated, making it difficult to effectively remove oxygen-containing silanes and alkali metal ions.

Method used

Under the protection of inert gas, dimethyldichlorosilane reacts with alkali metal in benzene solvent, then alcohols are neutralized and filtered, and the oxygen-containing silane is evaporated at high temperature, solid-liquid separation is performed using a cleaning solvent, and high-temperature evaporation and cleaning are repeated. , reduce the content of oxygen-containing silanes and alkali metal ions.

Benefits of technology

Effectively reduce the oxygen-containing silane and alkali metal ion content of polydimethylsilane, with oxygen content less than 0.6% and alkali metal content less than 30ppm, improving the high-temperature anti-oxidation and mechanical properties of silicon carbide ceramics, and simplifying the cleaning process .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a low-oxygen polydimethylsilane and a preparation method thereof, the preparation method comprising the following steps: under the protection of an inert gas, dimethyldichlorosilane and an alkali metal are added to a benzene solvent, reacted at high temperature to obtain a product; alcohols are added to the product, unreacted raw materials are neutralized, and then filtered to obtain a crude polydimethylsilane; the crude polydimethylsilane is evaporated at high temperature to remove oxygen-containing silane; the product after high-temperature evaporation is cleaned with a cleaning solvent and solid-liquid separation is performed; the solid-phase product of the solid-liquid separation is evaporated at high temperature, and the oxygen-containing silane is removed again to obtain the low-oxygen polydimethylsilane. The method can effectively reduce the oxygen-containing silane and alkali metal ion content of the polydimethylsilane, the oxygen content is less than 0.6%, and the alkali metal content is less than 30ppm, and low-oxygen polycarbosilane can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polydimethylsilane preparation, and particularly relates to low-oxygen polydimethylsilane and a preparation method thereof. Background Art

[0002] Polycarbosilane has important uses in many fields such as organic semiconductor devices, functional materials, and medicine. Polycarbosilane is an important precursor material for the preparation of silicon carbide ceramics. The lower the oxygen content and impurity content of polycarbosilane, the better the high-temperature oxygen resistance and mechanical properties of the prepared silicon carbide ceramics. Especially in the preparation of silicon carbide fibers, the lower the oxygen content in the precursor material, the better, and the less impurity content, the better. Polydimethylsilane is a precursor material for the preparation of polycarbosilane. The oxygen content and impurity content of polydimethylsilane have a direct impact on the high-temperature oxygen resistance and mechanical properties of silicon carbide ceramics.

[0003] Polydimethylsilane is a polymer material that is insoluble in organic or inorganic solvents and is an infusible solid with a cracking temperature above 300°C. At present, the preparation of polydimethylsilane mainly adopts the method of Wurtz reaction between chlorosilanes and alkali metals. After the reaction is completed, there will still be a lot of reaction raw materials in the system. For this reason, alcohols are usually added for neutralization, but more oxygen-containing silanes will be produced after neutralization. In addition, impurities such as chloride ions and alkali metal ions are also present in the reaction product. In order to remove impurities, filtering and washing are usually used. Because polydimethylsilane is an insoluble polymer powder, it cannot pass through the filter, while impurities such as oxygen-containing silane, chloride ions, and alkali metal ions can be dissolved in the solvent and pass through the filter, so they can be separated by filtering. The Chinese patent document with publication number CN 112538165 A discloses a polydimethylsilane material and a preparation method thereof. The preparation method uses the method of electrolyzing sodium chloride to prepare metallic sodium, and the obtained metallic sodium reacts with dimethyldichlorosilane. After the product is obtained, the product is neutralized with anhydrous ethanol, and then sodium chloride is extracted by evaporation. The extracted sodium chloride is recycled, and the remaining product is filtered, washed with water and ethanol, and then dried to obtain the finished product polydimethylsilane. However, dimethyldimethoxysilane or dimethyldiethoxysilane is generated after the alcohol neutralization product, and water is directly used for washing. Both oxygen-containing silane byproducts are hydrolyzed to generate dimethylsilanediol, and dimethylsilanediol is further polycondensed to generate complex siloxanes. Polydimethylsilane and oxygen-containing silane are usually wrapped around each other in crude polydimethylsilane, and the crude polydimethylsilane is cleaned with pure water and ethanol, and impurities are removed by filtering. Due to the low density of polydimethylsilane, the polydimethylsilane wraps the oxygen-containing silane and floats on the surface of the cleaning solvent during cleaning, resulting in poor cleaning effect. After filtration, part of the oxygen-containing silane is still wrapped in the polydimethylsilane, and the oxygen-containing silane has an oily hydrophobic structure, which wraps on the surface of the polydimethylsilane and blocks water from entering the interior to dissolve the alkali metal ions. Therefore, the cleaning process is complicated. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a low-oxygen polydimethylsilane and a preparation method thereof, which can effectively reduce the oxygen-containing silane and alkali metal ion content of polydimethylsilane, with the oxygen content being lower than 0.6% and the alkali metal content being lower than 30 ppm, and can prepare low-oxygen polycarbosilane.

[0005] In order to solve the above problems, one aspect of the present invention provides a method for preparing low-oxygen polydimethylsilane, comprising the following steps:

[0006] S1. Under the protection of an inert gas, dimethyldichlorosilane and an alkali metal are added to a benzene solvent and reacted at a high temperature to obtain a product;

[0007] S2. adding alcohols to the product to neutralize the unreacted raw materials, and then filtering to obtain crude polydimethylsilane;

[0008] S3. The crude polydimethylsilane is evaporated at high temperature to remove oxygen-containing silane;

[0009] S4. The product after high temperature evaporation is washed with a cleaning solvent and solid-liquid separation;

[0010] S5. The solid phase product of the solid-liquid separation is evaporated at high temperature to remove the oxygen-containing silane again to obtain low-oxygen polydimethylsilane.

[0011] Preferably, in step S3, the temperature during high-temperature evaporation is 80-250° C., and the pressure is normal pressure or vacuum.

[0012] Preferably, in step S5, the temperature during high-temperature evaporation is 60-250° C., and the pressure is normal pressure or vacuum.

[0013] Preferably, step S4 further comprises washing the solid phase product obtained by solid-liquid separation again with a washing solvent, and performing solid-liquid separation, and repeating the above washing and separation steps multiple times.

[0014] Preferably, in step S4, during the multiple washings, the washing solvent is pure water in at least one washing.

[0015] Preferably, in step S4, when pure water is used for the first cleaning, the mass ratio of pure water to dimethyldichlorosilane is 1:0.2-0.5.

[0016] Preferably, in step S1, the molar ratio of dimethyldichlorosilane to alkali metal is 1:1.9-2.1.

[0017] Preferably, in step S1, the reaction temperature when performing the reaction at high temperature is 70-120°C.

[0018] Preferably, in step S1, the alkali metal is sodium or potassium.

[0019] Another aspect of the present invention provides low-oxygen polydimethylsilane prepared by the above preparation method.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The preparation method of low-oxygen polydimethylsilane of the present invention utilizes the difference between the boiling point of the byproduct oxygen-containing silane and the cracking temperature of polydimethylsilane to remove the oxygen-containing silane by high-temperature evaporation, so that the oxygen-containing silane in the polydimethylsilane can be well removed to reduce the oxygen content of the product. In addition, the oxygen-containing silane is removed before the solvent is used for cleaning. On the one hand, the complicated side reaction after the hydrolysis of the oxygen-containing silane is avoided, and the generation of new by-products is avoided. On the other hand, after removing part of the oxygen-containing silane, the oxygen-containing silane encapsulating the polydimethylsilane is reduced, and the cleaning solvent is more likely to wet the polydimethylsilane for cleaning.

[0022] The method for preparing low-oxygen polydimethylsilane according to the embodiment of the present invention can effectively reduce the oxygen-containing silane and alkali metal ion content of polydimethylsilane, with the oxygen content being lower than 0.6% and the alkali metal content being lower than 30 ppm, and low-oxygen polycarbosilane can be prepared. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] A first aspect of an embodiment of the present invention provides a method for preparing low-oxygen polydimethylsilane, comprising the following steps:

[0025] S1. Under the protection of an inert gas, dimethyldichlorosilane and an alkali metal are added to a benzene solvent and reacted at a high temperature to obtain a product;

[0026] S2. adding alcohols to the product to neutralize the unreacted raw materials, and then filtering to obtain crude polydimethylsilane;

[0027] S3. The crude polydimethylsilane is evaporated at high temperature to remove oxygen-containing silane;

[0028] S4. The product after high temperature evaporation is washed with a cleaning solvent and solid-liquid separation;

[0029] S5. The solid phase product of the solid-liquid separation is evaporated at high temperature to remove the oxygen-containing silane again to obtain low-oxygen polydimethylsilane.

[0030] The preparation method of low oxygen-containing polydimethylsilane of the embodiment of the present invention, after step S1, polydimethylsilane, alkali metal chloride, unreacted dimethyldichlorosilane and alkali metal are obtained, and after step S2, dimethyldichlorosilane and alkali metal are neutralized, a mixture of product polydimethylsilane, alkali metal chloride, alkali metal alcoholate, residual alcohols and oxygen-containing silane is obtained. The oxygen-containing silane by-product is mainly dimethyldimethoxysilane or dimethyldiethoxysilane. The mixture is filtered to obtain a crude polydimethylsilane containing alkali metal chloride, alkali metal alcoholate and part of the oxygen-containing silane. Since the boiling point of dimethyldimethoxysilane is 81.4°C, the boiling point of dimethyldiethoxysilane is 114°C, and the cracking temperature of polydimethylsilane is above 300°C, dimethyldimethoxysilane or dimethyldiethoxysilane can be removed by high-temperature evaporation. Then, a cleaning solvent is added for cleaning, solid-liquid separation is performed, and the alkali metal compound is dissolved in the cleaning solvent and removed, and then high-temperature evaporation is performed again to remove the remaining small amount of cleaning solvent and oxygen-containing silane to obtain low-oxygen polydimethylsilane.

[0031] The method for preparing low-oxygen polydimethylsilane of the embodiment of the present invention utilizes the difference between the boiling point of the byproduct oxygen-containing silane and the cracking temperature of polydimethylsilane to remove the oxygen-containing silane by high-temperature evaporation, which can effectively remove the oxygen-containing silane in the polydimethylsilane and reduce the oxygen content of the product. In addition, removing the oxygen-containing silane before using the solvent for cleaning, on the one hand, avoids the complex side reactions after the hydrolysis of the above-mentioned oxygen-containing silane and avoids the generation of new by-products. On the other hand, after removing part of the oxygen-containing silane, the oxygen-containing silane encapsulating the polydimethylsilane is reduced, and the cleaning solvent is easier to wet the polydimethylsilane for cleaning. The method for preparing low-oxygen polydimethylsilane of the embodiment of the present invention can effectively reduce the content of oxygen-containing silane, chloride ion and alkali metal ion in polydimethylsilane.

[0032] In some embodiments, in step S3, during high-temperature evaporation, the byproduct dimethyldimethoxysilane or dimethyldiethoxysilane needs to be evaporated, and the structure of polydimethylsilane is not destroyed. Preferably, the temperature during high-temperature evaporation is 80 to 250°C, and the pressure is normal pressure or vacuum. In this temperature range, the alcohols and oxygen-containing silanes that are not filtered out can be evaporated and removed. Too high a temperature will destroy the structure of polydimethylsilane and produce other impurities. Further preferably, the temperature during high-temperature evaporation is 180 to 250°C.

[0033] In some embodiments, in step S3, when evaporating at high temperature, the evaporation time is 3-20 hours. Preferably, when evaporating at high temperature, the evaporation time is 20 hours.

[0034] In some embodiments, in step S5, during high-temperature evaporation, the byproduct oxygen-containing silane and the cleaning solvent remaining in the polydimethylsilane need to be evaporated and removed, and the structure of the polydimethylsilane is not destroyed. Preferably, the temperature during high-temperature evaporation is 60 to 250°C, and the pressure is normal pressure or vacuum. In this temperature range, the cleaning solvent and oxygen-containing silane that are not filtered out can be evaporated and removed. Further preferably, the temperature during high-temperature evaporation is 200 to 250°C.

[0035] In some embodiments, in step S5, when evaporating at high temperature, the evaporation time is 3-20 hours. Preferably, when evaporating at high temperature, the evaporation time is 20 hours.

[0036] In some embodiments, in steps S3 and S5, the mixture is fully tumbled during high-temperature evaporation.

[0037] In some embodiments, in steps S3 and S5, during high-temperature evaporation, evaporation is performed under a vacuum state.

[0038] In some embodiments, step S4 further includes washing the solid phase product of solid-liquid separation with a washing solvent again, and performing solid-liquid separation, and repeating the above-mentioned washing and separation steps multiple times. By washing, the alkali metal compound in the polydimethylsilane is dissolved in the washing solvent and removed by filtration. Multiple washings can make the alkali metal content in the polydimethylsilane lower. Preferably, in step S4, the product after high temperature evaporation is washed with a washing solvent, and the solid-liquid separation is performed for no less than 5 times.

[0039] In some embodiments, in step S4, the cleaning solvent can be any solvent that can effectively dissolve the alkali metal compound. Preferably, in the multiple cleanings, the cleaning solvent is pure water in at least one cleaning.

[0040] In some embodiments, in step S4, the multiple washings may use the same washing solvent or different washing solvents. Preferably, the multiple washings use different types of washing solvents. Specifically, in the multiple washings, organic solvents and inorganic solvents are used for washing respectively. The organic solvent may be alcohols, benzene, tetrahydrofuran, etc. The inorganic solvent may be pure water. For example, pure water is used for the first time, tetrahydrofuran is used for the second time, and pure water is used for the third time. In order to better remove the alkali metal compound, pure water is used for washing at least once in the multiple washings.

[0041] In some embodiments, in step S4, when pure water is used for washing for the first time, the mass ratio of pure water to dimethyldichlorosilane is greater than 1:0.5. Since crude polydimethylsilane contains a large amount of alkali metal chloride, and according to the solubility of alkali metal chloride in pure water, in order to ensure that the alkali metal chloride is fully dissolved and separated, it is preferred to further limit the mass ratio of water to the reaction raw material to a mass ratio greater than 1:0.5. Further preferably, in step S4, when pure water is used for washing for the first time, the mass ratio of pure water to dimethyldichlorosilane is 1:0.2 to 0.5.

[0042] In some embodiments, the molar ratio of dimethyldichlorosilane to alkali metal in step S1 is 1:1.9 to 2.1. Within this molar ratio range of the reactants, the conversion rate of the reaction between the two can be higher, the yield of the product polydimethylsilane can be higher, and the residual dimethyldichlorosilane and alkali metal can be less.

[0043] In some embodiments, in step S1, the reaction temperature when the reaction is carried out at high temperature is 70-120° C. Within this reaction temperature range, the conversion rate of the reaction of the two can be higher, the yield of the product polydimethylsilane can be higher, and the residual dimethyldichlorosilane and alkali metal can be less.

[0044] In some embodiments, in step S1, the alkali metal is sodium or potassium.

[0045] In some embodiments, the benzene solvent is toluene, xylene or a mixture of both.

[0046] In some embodiments, the alcohol is methanol, ethanol, or a mixture of the two.

[0047] Another aspect of the embodiments of the present invention provides low-oxygen polydimethylsilane prepared by the above-mentioned preparation method.

[0048] Example 1

[0049] A method for preparing low-oxygen polydimethylsilane in this embodiment comprises the following steps:

[0050] S1. Under N2 protection, 100 kg of dimethyldichlorosilane was dissolved in 200 L of xylene, 36 kg of metallic sodium was added at 115 °C, and the reaction was continued for 36 hours to obtain the product;

[0051] S2. 100 kg of ethanol was added to the product to neutralize the unreacted raw material, and then filtered to obtain crude polydimethylsilane;

[0052] S3. The crude polydimethylsilane was evaporated at 180°C for 10 h to remove oxygen-containing silane;

[0053] S4. The product after high temperature evaporation was washed with 250 kg of pure water, and then filtered to obtain a solid phase component filtered once, and then washed with 150 kg of pure water to obtain a second filtered solid phase component, and then washed with 150 kg of pure water to obtain a third filtered solid phase component to remove alkali metal compounds;

[0054] S5. The solid phase components obtained by three filtrations were evaporated at 180° C. for 10 h to remove residual water and oxygen-containing silane to obtain low-oxygen polydimethylsilane.

[0055] Example 2

[0056] A method for preparing low-oxygen polydimethylsilane in this embodiment comprises the following steps:

[0057] S1. Under N2 protection, 100 kg of dimethyldichlorosilane was dissolved in 200 L of xylene, 36 kg of metallic sodium was added at 115 °C, and the reaction was continued for 36 hours to obtain the product;

[0058] S2. 100 kg of ethanol was added to the product to neutralize the unreacted raw material, and then filtered to obtain crude polydimethylsilane;

[0059] S3. Evaporate the crude polydimethylsilane at 180°C and -0.1MPa vacuum for 10h to remove oxygen-containing silane;

[0060] S4. The product after high temperature evaporation was washed with 250 kg of pure water, and then filtered to obtain a solid phase component filtered once, and then washed with 150 kg of pure water to obtain a second filtered solid phase component, and then washed with 150 kg of pure water to obtain a third filtered solid phase component to remove alkali metal compounds;

[0061] S5. The solid phase components obtained by three filtrations were evaporated at 180°C and -0.1 MPa vacuum for 10 h to remove residual water and oxygen-containing silane to obtain low-oxygen polydimethylsilane.

[0062] Example 3

[0063] A method for preparing low-oxygen polydimethylsilane in this embodiment comprises the following steps:

[0064] S1. Under N2 protection, 100 kg of dimethyldichlorosilane was dissolved in 200 L of xylene, 36 kg of metallic sodium was added at 115 °C, and the reaction was continued for 36 hours to obtain the product;

[0065] S2. 100 kg of methanol was added to the product to neutralize the unreacted raw material, and then filtered to obtain crude polydimethylsilane;

[0066] S3. The crude polydimethylsilane was evaporated at 180°C for 10 h to remove oxygen-containing silane;

[0067] S4. The product after high temperature evaporation was washed with 250 kg of pure water, and then filtered to obtain a solid phase component filtered once, and then washed with 150 kg of pure water to obtain a second filtered solid phase component, and then washed with 150 kg of pure water to obtain a third filtered solid phase component to remove alkali metal compounds;

[0068] S5. The solid phase components obtained by three filtrations were evaporated at 180° C. for 10 h to remove residual water and oxygen-containing silane to obtain low-oxygen polydimethylsilane.

[0069] Example 4

[0070] A method for preparing low-oxygen polydimethylsilane in this embodiment comprises the following steps:

[0071] S1. Under N2 protection, 100 kg of dimethyldichlorosilane was dissolved in 200 L of xylene, 36 kg of metallic sodium was added at 115 °C, and the reaction was continued for 36 hours to obtain the product;

[0072] S2. 100 kg of methanol was added to the product to neutralize the unreacted raw material, and then filtered to obtain crude polydimethylsilane;

[0073] S3. The crude polydimethylsilane was evaporated at 180°C for 10 h to remove oxygen-containing silane;

[0074] S4. The product after high temperature evaporation was washed with 250 kg of pure water, and then filtered to obtain a solid phase component filtered once, and then washed with 150 kg of tetrahydrofuran, and then filtered to obtain a second filtered solid phase component, and then washed with 150 kg of pure water to obtain a third filtered solid phase component to remove alkali metal compounds;

[0075] S5. The solid phase components obtained by three filtrations were evaporated at 180° C. for 10 h to remove residual water and oxygen-containing silane to obtain low-oxygen polydimethylsilane.

[0076] Example 5

[0077] The preparation method of low-oxygen polydimethylsilane in this embodiment is the same as that in Example 3 in other steps, except that in steps S3 and S5, the evaporation temperature is 100° C. and the evaporation time is 10 h.

[0078] Example 6

[0079] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in steps S3 and S5, the evaporation temperature is 250° C. and the evaporation time is 10 h.

[0080] Example 7

[0081] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in steps S3 and S5, the evaporation temperature is 280° C. and the evaporation time is 10 h.

[0082] Example 8

[0083] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in steps S3 and S5, the evaporation temperature is 180° C. and the evaporation time is 20 h.

[0084] Example 9

[0085] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in steps S3 and S5, the evaporation temperature is 180° C., the evaporation time is 10 h, and the evaporation pressure is -0.1 MPa.

[0086] Example 10

[0087] The preparation method of low-oxygen polydimethylsilane in this embodiment is the same as that in Example 3 in other steps, except that in step S4, 150 kg of pure water, 150 kg of pure water, and 150 kg of pure water are used for three washings respectively.

[0088] Embodiment 11

[0089] The preparation method of low-oxygen polydimethylsilane in this embodiment is the same as that in Example 3 in other steps, except that in step S4, 200 kg of pure water, 150 kg of pure water, and 150 kg of pure water are used for three washings respectively.

[0090] Example 12

[0091] The preparation method of low-oxygen polydimethylsilane in this embodiment is the same as that in Example 3 in other steps, except that in step S4, 500 kg of pure water, 150 kg of pure water, and 150 kg of pure water are used for three washings respectively.

[0092] Example 13

[0093] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in step S4, five washings are performed using 250 kg of pure water, 150 kg of pure water, 150 kg of pure water, 150 kg of pure water, and 150 kg of pure water, respectively.

[0094] Embodiment 14

[0095] The preparation method of low-oxygen polydimethylsilane in this embodiment has the same other steps as those in Example 3, except that in step S4, five washings are performed using 250 kg of pure water, 150 kg of tetrahydrofuran, 150 kg of tetrahydrofuran, 150 kg of pure water, and 150 kg of pure water, respectively.

[0096] The three cleanings in Examples 1-3 all use pure water, which is better than the cleaning method of pure water, tetrahydrofuran, pure water, inorganic solvent, and organic solvent combined in Example 4. The effect of removing sodium ions is better, and Example 4 has a better removal effect on oxygen-containing silanes. Compared with Examples 3, 5, 6, and 7, the difference is the evaporation temperature. In comparison, the evaporation temperature of Example 6 is more suitable. The higher the evaporation temperature, the better the removal effect of oxygen-containing silanes. However, after the evaporation temperature exceeds a certain value, the increased temperature can no longer significantly remove oxygen-containing silanes, and some products begin to crack. Compared with Examples 3 and 8, the difference is the evaporation time. In comparison, the longer the evaporation time, the better the removal effect of oxygen-containing silanes. Compared with Examples 3 and 9, the difference is the evaporation pressure. In comparison, the lower the vacuum degree during evaporation, the better the removal effect of oxygen-containing silanes. Compared with Examples 3, 10, 11, and 12, the difference is that the amount of pure water used for the first water cleaning is different. In comparison, the more pure water, the better the removal effect of sodium ions. The preferred mass ratio of water to dimethyldichlorosilane is 1:0.2-0.5. Compared with Examples 3, 13, and 14, the difference is that the number of cleaning times of inorganic solvents and organic solvents is increased respectively. The more cleaning times of inorganic solvent pure water, the better the removal effect of sodium ions, and the more cleaning times of organic solvents, the better the removal effect of oxygen-containing silane.

[0097] Performance Indicators Oxygen content% Sodium ion content ppm Example 1 0.6 28 Example 2 0.5 28 Example 3 0.6 27 Example 4 0.4 76 Example 5 1.8 30 Example 6 0.5 27 Example 7 0.5 28 Example 8 0.4 29 Example 9 0.4 28 Example 10 0.6 56 Embodiment 11 0.6 42 Example 12 0.6 21 Example 13 0.6 8 Embodiment 14 0.2 25

[0098] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing low-oxygen polydimethylsilane, characterized in that: The following steps are involved: S1. Under the protection of an inert gas, dimethyldichlorosilane and an alkali metal are added to a benzene solvent, and the reaction is carried out at a high temperature, the reaction temperature is 70 to 120° C., and the molar ratio of dimethyldichlorosilane to the alkali metal is 1:1.9 to 2.1 to obtain a product; S2. adding alcohols to the product to neutralize the unreacted raw materials, and then filtering to obtain crude polydimethylsilane; S3. The crude polydimethylsilane is evaporated at high temperature to remove oxygen-containing silane, the temperature of the high temperature evaporation is 180 to 250 ° C, and the pressure of the high temperature evaporation is vacuum; S4. The product after high-temperature evaporation is washed with a cleaning solvent and solid-liquid separation is performed, and the solid-liquid separation solid phase product is washed with a cleaning solvent, and solid-liquid separation is performed, and the above-mentioned cleaning and separation steps are repeated multiple times, and the cleaning solvent is pure water during at least one of the multiple washings. When pure water is used for the first washing, the mass ratio of pure water to dimethyldichlorosilane is 1:0.2 to 0.5; S5. The solid phase product of the solid-liquid separation is evaporated at high temperature to remove the oxygen-containing silane again, wherein the temperature of the high temperature evaporation is 180 to 250° C. and the pressure of the high temperature evaporation is vacuum, to obtain low-oxygen polydimethylsilane.

2. The method for preparing low-oxygen polydimethylsilane according to claim 1, characterized in that: In step S1, the alkali metal is sodium or potassium.

3. Low-oxygen polydimethylsilane prepared by the preparation method as claimed in claim 1 or 2.