Compound alkali-aggregate reaction crack bottom glaze, compound alkali-aggregate reaction crack tile and preparation method thereof
Through the compound alkali aggregate reaction, cracks in the bottom release layer are formed and the cracks are hidden under the protective release layer, which solves the problems of upturned bricks and easy accumulation of dirt and grime caused by traditional crack glaze, and achieves cracks with high flatness and pollution resistance. Ceramic tiles, suitable for applications in the field of architectural ceramics.
Patent Information
- Application Number
- CN202410935453.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The cracks caused by the difference in expansion coefficient of traditional cracked glaze cause the ceramic tiles to warp and easily trap dirt and evil, making it difficult to be used in the field of architectural ceramics.
The compound alkali aggregate reaction crack base glaze is used, which naturally cracks during the drying process through alkali-silicate and alkali-carbonate reactions, forming cracks in the base glaze layer, and hiding the cracks under the protective glaze layer to avoid glaze cracks. Ensure brick surface flatness and pollution resistance.
Cracked tiles with no cracks and high flatness are realized, which avoids the problems of upturned tiles and easy trapping of dirt and evil, and is suitable for factory mass production.
Smart Images

Figure CN118495813B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building ceramics, and in particular relates to a compound alkali-aggregate reaction crack bottom glaze, a compound alkali-aggregate reaction crack ceramic tile and a preparation method thereof. Background Art
[0002] Ceramics has a long history and has become an indispensable building decoration material in people's home life. In particular, the rise of ceramic rock slabs in recent years has shown great development potential in the home furnishing field. In the long development process, many types of ceramic art glazes have emerged, such as crystal glaze, kiln-changed glaze, color-changing glaze, pearl glaze, iridescent glaze, rhyme glaze, etc., all of which are treasures among ceramic glazes. However, ceramic art glazes are rarely used in the architectural ceramics industry, mainly because architectural ceramics not only require excellent wear resistance and pollution resistance, but also require extremely high surface flatness. These harsh conditions restrict the application of ceramic art glazes.
[0003] Among ceramic art glazes, there is a special glaze called crackle glaze. Cracks were originally a defect in the porcelain making process. However, the cracks on the glaze of some products are very special, with uniform and clear lines covering the entire surface, giving people a special sense of beauty. Inspired by this, people consciously prepared this kind of glaze cracks, thus creating crackle glaze. The glaze of porcelain prepared with crackle glaze is covered with many small cracks, resembling cracks, crab claws or ice cracks. Crackle glaze has become a classic in artistic ceramics due to its unique visual effects, especially the Ge Kiln porcelain of the Song Dynasty, which has left a strong color in the long river of history.
[0004] The reason for the crackle glaze is that the expansion coefficient of the glaze is greater than that of the body. During the cooling process, the glaze surface produces a large tensile stress, which causes the glaze surface to crack and form many cracks. However, at the same time, because the expansion coefficient of the glaze is greater than that of the body, the tile shape will be warped, which is not conducive to the production and laying of tiles. In addition, because the cracks are located on the surface of the glaze layer, it is very easy to harbor dirt and grime, which greatly reduces the service life of the tile. Therefore, due to its generation mechanism and the physical characteristics of the surface cracks, traditional crackle glaze cannot be used in the field of architectural ceramics. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a compound alkali-aggregate reaction cracked base glaze, a compound alkali-aggregate reaction cracked ceramic tile and a preparation method thereof. The present invention abandons the idea that the traditional cracked glaze relies on the difference in expansion coefficients of the body and glaze to cause cracks, and develops a special compound alkali-aggregate reaction cracked base glaze, which generates cracks by a compound alkali-aggregate reaction. When the base glaze is applied to the production of ceramic tiles, a cracked ceramic tile with no surface cracks, uniform cracks in the base glaze layer and extremely high tile surface flatness is obtained after high-temperature firing.
[0006] In the first aspect, the present invention provides a compound alkali-aggregate reaction crack enamel. The mineral composition of the compound alkali-aggregate reaction crack enamel includes basic minerals and added alkaline raw materials; wherein the basic minerals include, by mass percentage: quartz 10-20%, calcined alumina 5-10%, potassium feldspar 20-30%, kaolin 5-15%, calcined kaolin 5-15%, zirconium silicate 5-10%, argillaceous dolomite 10-20%, amorphous silicon dioxide 5-20%; the alkaline raw materials account for 0.5-1.0% of the total mass of the basic minerals.
[0007] Preferably, the alkaline raw material is sodium carbonate. In addition to increasing the pH value of the glaze slurry, sodium carbonate can also be used as a glaze slurry suspending agent and a degumming agent to improve the glaze slurry suspension performance.
[0008] Preferably, the chemical composition of the compound alkali-aggregate reaction crack bottom glaze includes, by mass percentage, loss on ignition: 4-6%, SiO 2 :56~72%,Al 2 O 3 :14~30%, K 2 O: 2~5%, Na 2 O: 1~2%, CaO: 2~9%, MgO: 0.5~2%, ZrO 2 : 2.5~10%.
[0009] In a second aspect, the present invention provides a method for preparing a composite alkali-aggregate reaction cracked tile. The preparation method comprises the following steps:
[0010] Applying the compound alkali-aggregate reaction crackle base glaze on the surface of the body;
[0011] Inkjet printing patterns on the surface of the body after applying the composite alkali-aggregate reaction crackle base glaze;
[0012] Applying protective glaze on the surface of the blank after the inkjet printing pattern;
[0013] The green body with protective glaze applied is fired and polished to obtain the composite alkali-aggregate reaction crack ceramic tile.
[0014] Preferably, the compound alkali-aggregate reaction crack base glaze is applied by pouring glaze or spraying glaze.
[0015] Preferably, the chemical composition of the protective glaze includes, by mass percentage: loss on ignition: 5.1-8.7%, SiO 2 :40~60%,Al 2 O 3 : 15~20%, CaO: 2~10%, MgO: 1~3%, K 2 O: 2~6%, Na 2O: 1~3%, ZnO: 1~5%, BaO: 1~4%, SrO: 0.5~3.0%.
[0016] Preferably, the protective glaze is applied by pouring glaze or spraying glaze.
[0017] Preferably, the sintering temperature is 1180-1230° C., and the sintering time is 40-70 minutes.
[0018] In a third aspect, the present invention provides a compound alkali-aggregate reaction crack ceramic tile, which is obtained according to the preparation method.
[0019] Beneficial Effects
[0020] 1. The composite alkali-aggregate reaction cracked ceramic tile obtained by the preparation method of the present invention has a flat brick shape, thus avoiding the problem of the traditional cracked glaze ceramic tile being prone to warping.
[0021] 2. The cracks produced in the compound alkali-aggregate reaction cracked ceramic tile obtained by the preparation method of the present invention are under the protective glaze layer, providing a visual effect of cracked glaze, but there are no cracks on the surface of the glaze layer. Therefore, the cracked ceramic tile has excellent pollution resistance and avoids the problem that traditional cracked glaze ceramic tiles are easy to hide dirt and are difficult to clean.
[0022] 3. The production process of the composite alkali-aggregate reaction cracked ceramic tiles of the present invention is suitable for factory batch production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a detailed rendering of the brick surface of Example 1 of the present invention;
[0024] Figure 2 This is a detailed rendering of the brick surface of Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0025] The present invention is further described by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention. The following is an exemplary description of the compound alkali-aggregate reaction crack bottom glaze, compound alkali-aggregate reaction crack tile and the preparation method thereof according to the present invention.
[0026] The green body powder is pressed into a shape to obtain a green body. The chemical composition of the green body powder is not limited, and the green body powder commonly used in the art can be used. In some embodiments, the chemical composition of the green body powder includes: SiO 2 :63~67%,Al 2 O 3 :18~23%,Fe 2 O 3 :0.1~0.5%,TiO 2: 0~0.2%, CaO: 0.1~4.0%, MgO: 0.5~1.5%, K 2 O: 2.0~3.5%, Na 2 O: 2.0~3.5%, loss on ignition: 3.5~5.5%.
[0027] The green body is dried. The drying temperature and drying time can be adjusted as needed. For example, the drying temperature can be 100-150°C, and the drying time can be 50-75 minutes. The moisture content of the green body after drying is preferably controlled within 0.5wt%.
[0028] Preparation of compound alkali aggregate reaction crackle base glaze.
[0029] As an example, the mineral composition of the compound alkali-aggregate reaction crack enamel includes basic minerals and added alkaline raw materials, wherein the basic mineral composition includes by mass percentage: quartz 10-20%, calcined alumina 5-10%, potassium feldspar 20-30%, kaolin 5-15%, calcined kaolin 5-15%, zirconium silicate 5-10%, argillaceous dolomite 10-20%, amorphous silicon dioxide 5-20%. The proportion of added sodium carbonate to the total mass of the basic minerals is 0.5-1.0%. The amorphous silicon dioxide and argillaceous dolomite of the compound alkali-aggregate reaction crack enamel react with other raw materials under alkaline conditions, respectively, so that the glaze naturally cracks during the drying process, and cracks can be formed without forming a large difference in expansion coefficient with the blank. At the same time, the compound alkali-aggregate reaction crack enamel can also play a role in covering the base color defects of the blank and promoting the color of the inkjet pattern.
[0030] As an example, the chemical composition of argillaceous dolomite includes, in mass percentage: SiO 2 :18.89%,Al 2 O 3 :12.70%,Fe 2 O 3 :0.45%, TiO 2 :0.08%, CaO: 28.40%, MgO: 6.13%, K 2 O: 0.89%, Na 2 O: 0.20%, loss on ignition: 32.26%.
[0031] According to the mineral composition of the above-mentioned compound alkali-aggregate reaction crack bottom glaze, weigh the raw materials, add sodium carboxymethyl cellulose, sodium tripolyphosphate and water, put them into a ball mill, and ball-mill until the residue after passing through a 325-mesh sieve is 0.3-0.8wt%. The ball-milled glaze slurry is sieved, iron-removed and aged to obtain a compound alkali-aggregate reaction crack bottom glaze slurry. The aging time can be 24-48 hours. For example, sodium carboxymethyl cellulose can account for 0.1-0.5wt% of the mineral composition of the compound alkali-aggregate reaction crack bottom glaze, sodium tripolyphosphate can account for 0.3-1.5wt% of the mineral composition of the compound alkali-aggregate reaction crack bottom glaze, and water can account for 35-50wt% of the mineral composition of the compound alkali-aggregate reaction crack bottom glaze. During use, water can be added to adjust the specific gravity of the bottom glaze to obtain the final required specific gravity of the compound alkali-aggregate reaction crack bottom glaze.
[0032] In some embodiments, the chemical composition of the compound alkali-aggregate reaction crack bottom glaze includes, by mass percentage: loss on ignition: 4-6%, SiO 2 :56~72%,Al 2 O 3 :14~30%, K 2 O: 2~5%, Na 2 O: 1~2%, CaO: 2~9%, MgO: 0.5~2%, ZrO 2 : 2.5~10%.
[0033] The double alkali-aggregate reaction crackle base glaze is applied on the surface of the dried green body. The double alkali-aggregate reaction crackle base glaze can be applied by pouring glaze or spraying glaze.
[0034] In some embodiments, the specific gravity of the compound alkali-aggregate reaction crack bottom glaze is 1.85-1.88 g / cm 3 , glaze application amount is 380~450 g / m 2 If the amount of compound alkali-aggregate reaction crack base glaze applied is too little, no cracks will appear and the covering effect will be poor; if the amount of compound alkali-aggregate reaction crack base glaze applied is too much, the moisture content introduced into the brick surface will be too high, causing the blank to explode when entering the kiln.
[0035] The pattern is inkjet printed on the surface of the body after the composite alkali-aggregate reaction crackle base glaze is applied. The pattern can be printed with ordinary ceramic ink. The color and texture of the inkjet printed pattern can be changed according to the layout design requirements. As an example, the pattern is a decorative pattern.
[0036] A protective glaze is applied on the surface of the blank after the inkjet printing pattern, and the protective glaze commonly used in the art can be used.
[0037] In some embodiments, the chemical composition of the protective glaze includes, by mass percentage: loss on ignition: 5.1-8.7%, SiO 2:40~60%,Al 2 O 3 : 15~25%, CaO: 2~10%, MgO: 1~3%, K 2 O: 2~6%, Na 2 O: 1~3%, ZnO: 1~5%, BaO: 1~4%, SrO: 0.5~3.0%.
[0038] As an example, the mineral composition of the protective glaze includes, by mass percentage, 30-50% potassium feldspar, 10-15% sodium feldspar, 5-15% calcite, 2-5% zinc oxide, 2-6% barium carbonate, 1-6% strontium carbonate, 5-10% washed kaolin, and 4-8% burned talc.
[0039] According to the mineral composition of the protective glaze, weigh the raw materials, add sodium carboxymethyl cellulose, sodium tripolyphosphate and water, put them into a ball mill, and ball-mill until the residue after passing through a 325-mesh sieve is 0.3-0.8wt%. The ball-milled glaze slurry is sieved, iron-removed and aged to obtain a protective glaze slurry. The aging time can be 24-48 hours. For example, sodium carboxymethyl cellulose can account for 0.1-0.5wt% of the mineral composition of the protective glaze, sodium tripolyphosphate can account for 0.3-1.5wt% of the mineral composition of the protective glaze, and water can account for 35-50wt% of the mineral composition of the protective glaze. During use, water can be added to adjust the specific gravity of the protective glaze to obtain the final required specific gravity of the protective glaze.
[0040] The protective glaze may be applied by pouring or spraying. In some embodiments, the specific gravity of the protective glaze is 1.82-1.88 g / cm 3 , application amount is 400~550 g / m 2 If the amount of protective glaze applied is too little, it will not be able to fully protect the underlying compound alkali-aggregate reaction crack base glaze, especially after polishing, the compound alkali-aggregate reaction crack base glaze layer may be exposed and affect the glaze quality. If the amount of protective glaze applied is too much, the gas generated by the glaze during the high-temperature firing stage is difficult to discharge, and defects such as pinholes and poor anti-fouling are prone to occur, which not only causes material consumption but also affects the glaze presentation effect.
[0041] The green body after the protective glaze is dried. It can be put into a drying kiln for drying. The drying temperature can be 100~150℃.
[0042] Firing. Put into kiln for firing. The firing temperature is 1180-1230°C and the firing time is 40-70 minutes.
[0043] Edge grinding and polishing. The polishing process commonly used in this field can be used. Polishing can be carried out in sequence by rough polishing, medium polishing, and fine polishing.
[0044] In summary, the present invention abandons the idea that traditional crack glaze relies on the difference in expansion coefficients of body and glaze to cause cracks, and develops a special compound alkali-aggregate reaction crack base glaze, which produces cracks by a compound alkali-aggregate reaction. When it is applied to the production of ceramic tiles, after high-temperature firing, a cracked ceramic tile with no cracks on the surface, uniform cracks in the base glaze layer and extremely high tile surface flatness is obtained.
[0045] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0046] Embodiment 1~5
[0047] A method for preparing a composite alkali-aggregate reaction cracked tile comprises the following steps:
[0048] Step 1. Press the green body powder into a green body and dry the green body.
[0049] Step 2. Weigh the mineral raw materials of the compound alkali aggregate reaction crack bottom glaze according to Table 1. Place the weighed raw materials into a ball mill, add 40wt% of water, 0.2wt% of sodium carboxymethyl cellulose, and 0.3wt% of sodium tripolyphosphate, which account for 40wt% of the mineral composition of the compound alkali aggregate reaction crack bottom glaze, and ball mill until the slurry has a sieve residue of 0.6wt% after passing through a 325-mesh sieve. Sieve the ball-milled glaze slurry, remove iron, and age it for 24 hours to obtain the slurry of the compound alkali aggregate reaction crack bottom glaze.
[0050] Step 3: Apply the compound alkali-aggregate reaction crackle base glaze on the ceramic body. The compound alkali-aggregate reaction crackle base glaze is applied by pouring glaze. The specific gravity of the compound alkali-aggregate reaction crackle base glaze is 1.85g / cm 3 , glaze application amount is 400 g / m 2 .
[0051] Step 4. Inkjet printing a pattern on the surface of the green body after applying the double alkali-aggregate reaction crackle base glaze.
[0052] Step 5. Apply protective glaze on the surface of the blank after the inkjet printing pattern. The chemical composition of the protective glaze includes, by mass percentage: loss on ignition: 6.4%, SiO 2 :49%,Al 2 O 3 :21.5%, CaO: 7.1%, MgO: 2.0%, K 2O: 3.5%, Na 2 O: 1.2%, ZnO: 3.8%, BaO: 2.5%, SrO: 3.0%. The protective glaze is applied by pouring glaze. The specific gravity of the protective glaze is 1.86g / cm 3 , glaze weight is 450 g / m 2 .
[0053] Step 6. Dry, sinter, grind and polish the green body after applying the protective glaze to obtain the composite alkali aggregate reaction crack ceramic tile. The sintering temperature is 1210° C. and the sintering time is 60 minutes.
[0054] Table 1 Mineral composition and experimental results of the compound alkali-aggregate reaction crack bottom glaze of each embodiment
[0055]
[0056] The cracks of the composite alkali-aggregate reaction crack ceramic tiles prepared in Examples 1 to 5 are natural and uniform, without glaze defects. Figure 1 This is a brick surface effect diagram of Example No. 1 of the present invention. It can be seen that the compound alkali-aggregate reaction crack tile obtained by the preparation method of the present invention has a flat brick shape, avoiding the problem of the traditional crack glaze tile brick shape warping. Moreover, the cracks produced by the compound alkali-aggregate reaction crack tile obtained by the preparation method of the present invention are under the protective glaze layer, providing a visual effect of crack glaze, but there are no cracks on the surface of the glaze layer.
[0057] Comparative Examples 1 to 5
[0058] A method for preparing a ceramic tile comprises the following steps:
[0059] Step 1. Press the green body powder into a green body and dry the green body.
[0060] Step 2. Weigh the mineral raw materials for the base glaze according to Table 2. The mineral composition of the base glaze includes basic minerals and additional alkaline raw materials (sodium carbonate). The alkaline raw materials account for 1.0~1.5% of the total mass of the basic minerals. Place the weighed raw materials in a ball mill, add 40wt% of water, 0.2wt% of sodium carboxymethyl cellulose, and 0.3wt% of sodium tripolyphosphate, which account for the mineral composition of the base glaze, and ball mill until the slurry has a sieve residue of 0.6wt% after passing through a 325-mesh sieve. Sieve the ball-milled glaze slurry, remove iron, and age it for 24 hours to obtain the base glaze slurry.
[0061] Step 3: Apply the base glaze on the ceramic body. The base glaze is applied by pouring. The specific gravity of the base glaze is 1.85g / cm 3 , glaze application amount is 400 g / m 2 .
[0062] Step 4. Inkjet print the pattern on the surface of the blank after applying the base glaze.
[0063] Step 5. Apply protective glaze on the surface of the blank after the inkjet printing pattern. The chemical composition of the protective glaze includes, by mass percentage: loss on ignition: 6.4%, SiO 2 :49%,Al 2 O 3 :21.5%, CaO: 7.1%, MgO: 2.0%, K 2 O: 3.5%, Na 2 O: 1.2%, ZnO: 3.8%, BaO: 2.5%, SrO: 3.0%. The protective glaze is applied by pouring glaze. The specific gravity of the protective glaze is 1.86g / cm 3 , glaze weight is 450 g / m 2 .
[0064] Step 6. Dry, fire, grind and polish the green body after applying the protective glaze to obtain a tile. The firing temperature is 1210° C. and the firing time is 60 minutes.
[0065] Table 2 Mineral composition and experimental results of the compound alkali-aggregate reaction crack bottom glaze of each comparative example
[0066]
[0067] The calcined alumina content of Comparative Example 1 is too high, resulting in the glaze firing temperature being too high. During high-temperature firing, there is less liquid phase and it is impossible to form a sufficient intermediate layer with the body, so the defect of glaze peeling occurs.
[0068] The potassium feldspar content in Comparative Example 2 is relatively high, resulting in the glaze firing temperature being too low. There is more liquid phase during high-temperature firing, and the high-temperature fluidity of the glaze is stronger. The glaze slurry will automatically fill the cracks during firing, so the final glaze surface is flat and smooth without any crack effect.
[0069] The argillaceous dolomite content of Comparative Example 3 is relatively low, resulting in insufficient content of specific carbonates necessary for the compound alkali-aggregate reaction, and failure to produce compound alkali-aggregate reaction cracks.
[0070] Figure 2 This is a brick surface effect diagram of comparative example 4 of the present invention. It can be seen that due to the high content of amorphous silica in comparative example 4, more free silica is generated during firing, and the thermal expansion coefficient of the glaze is larger, which causes the brick shape to warp up and the protective glaze layer to crack. Therefore, after firing, in addition to the compound alkali-aggregate reaction cracks in the bottom glaze layer, straight cracks also appear in the protective glaze layer, resulting in poor anti-fouling performance and mechanical properties of the tile.
[0071] The sodium carbonate content in Comparative Example 5 is relatively high. In addition to being used as a degumming agent, sodium carbonate can also act as a thixotropic agent. Too high a sodium carbonate content will cause the glaze slurry to be thixotropic, and the glaze fluidity will be greatly reduced, eventually resulting in abnormal defects such as dead slurry.
[0072] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-mentioned embodiments are exemplary and cannot be interpreted as limiting the present invention. Those of ordinary skill in the art can change, modify, replace and modify the above-mentioned implementation within the scope of the present invention.
Claims
1. A compound alkali aggregate reaction crack base glaze, It is characterized in that The mineral composition of the compound alkali aggregate reaction crackle base glaze includes basic minerals and added alkaline raw materials; wherein the basic minerals include, by mass percentage, quartz 10-20%, calcined alumina 5-10%, potassium feldspar 20-30%, kaolin 5-15%, calcined kaolin 5-15%, zirconium silicate 5-10%, argillaceous dolomite 10-20%, and amorphous silicon dioxide 5-20%; the alkaline raw materials account for 0.5-1.0% of the total mass of the basic minerals.
2. The compound alkali-aggregate reaction crack bottom glaze according to claim 1, It is characterized in that The alkaline raw material is sodium carbonate.
3. The compound alkali-aggregate reaction crack bottom glaze according to claim 1 or 2, It is characterized in that The chemical composition of the compound alkali-aggregate reaction crack bottom glaze includes, by mass percentage, loss on ignition: 4-6%, SiO 2 :56~72%,Al 2 O 3 :14~30%, K 2 O: 2~5%, Na 2 O: 1~2%, CaO: 2~9%, MgO: 0.5~2%, ZrO 2 : 2.5~10%.
4. A method for preparing composite alkali-aggregate reaction cracked tiles, It is characterized in that The preparation method comprises the following steps: Applying the compound alkali-aggregate reaction crackle base glaze according to any one of claims 1 to 3 on the surface of the body; Inkjet printing patterns on the surface of the body after applying the composite alkali-aggregate reaction crackle base glaze; Applying protective glaze on the surface of the blank after the inkjet printing pattern; The green body with protective glaze applied is fired and polished to obtain the composite alkali-aggregate reaction crack ceramic tile.
5. The preparation method according to claim 4, It is characterized in that The compound alkali-aggregate reaction crack base glaze is applied by pouring glaze or spraying glaze.
6. The preparation method according to claim 4, It is characterized in that The chemical composition of the protective glaze includes, by mass percentage: loss on ignition: 5.1-8.7%, SiO 2 :40~60%,Al 2 O 3 : 15~25%, CaO: 2~10%, MgO: 1~3%, K 2 O: 2~6%, Na 2 O: 1~3%, ZnO: 1~5%, BaO: 1~4%, SrO: 0.5~3.0%.
7. The preparation method according to claim 4, It is characterized in that The mineral composition of the protective glaze includes, by mass percentage, 30-50% potassium feldspar, 10-15% sodium feldspar, 5-15% calcite, 2-5% zinc oxide, 2-6% barium carbonate, 1-6% strontium carbonate, 5-10% washed kaolin, and 4-8% burned talc.
8. The preparation method according to claim 4, It is characterized in that The protective glaze is applied by pouring glaze or spraying glaze.
9. The preparation method according to claim 4, It is characterized in that The sintering temperature is 1180-1230° C., and the sintering time is 40-70 minutes.
10. A composite alkali-aggregate reaction cracked tile, It is characterized in that The compound alkali-aggregate reaction cracked ceramic tile is obtained according to the preparation method described in any one of claims 4 to 9.