Solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios and preparation method thereof
By optimizing the design of solid waste formula and reinforcing powder, combined with suppression and mineralization reaction technology, the problem of insufficient mechanical strength and impermeability of solid waste-based artificial stone is solved, achieving high pressure resistance and multi-scenario applicable mechanical strength and waterproofing. Performance improvements.
Patent Information
- Application Number
- CN202410955832.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The existing solid waste-based artificial stone has insufficient mechanical strength and impermeability properties, making it difficult to meet the needs of high-pressure and multi-scenario production and life.
By optimizing the solid waste formula system, a combination of calcium-containing solid waste powder, solid waste particles and reinforcing powder is used to control the gradation of solid waste particles and the proportions of hydrotalcite, isocyanate and modifiers to form a hydrophobically modified enhanced powder. Pressure and mineralization reaction technology improves the mechanical strength and waterproof performance of artificial stone.
It significantly improves the flexural strength, compressive strength and durability of artificial stone, reduces water absorption, effectively resists the invasion of external acid ions, and improves the weather resistance and compactness of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid waste-based artificial stones, and in particular to a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios and a preparation method thereof. Background Art
[0002] The mechanical strength of solid waste-based artificial stone is usually poor, and researchers in the field are committed to improving the compressive strength of artificial stone through different ways. For example, a Chinese patent application document (publication number CN115583820A) provides an inorganic artificial stone prepared by carbon dioxide curing and a preparation method thereof, using a carbon-fixed cementitious material as the cementitious material of the inorganic artificial stone, after being pressed and formed, it is placed in a carbon dioxide atmosphere at room temperature for curing, and an inorganic artificial stone product with excellent compressive resistance is prepared. A Chinese patent application document (publication number CN115340327A) provides a method for preparing a cast carbonized stone, using carbonized steel slag as fine aggregate and raw material, and carbonized steel slag provides a pore structure during the carbonization process. CO2 diffuses through the pores to the surrounding of the stone, increasing the carbonization degree of the plate, and the two carbonization processes absorb more carbon dioxide, which increases the strength of the stone. However, the mechanical strength and impermeability of artificial stone need to be further improved to meet people's production and living needs in multiple scenarios. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. By optimizing the solid waste formula system, the problems of poor mechanical strength and waterproof performance of existing solid waste-based artificial stones are solved to meet the actual needs of different application scenarios.
[0004] On the one hand, the present invention provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. The raw materials for its preparation include at least 30-80 parts of calcium-containing solid waste powder, 20-70 parts of solid waste particles, 1-8 parts of reinforcing powder, and 5-50 parts of water, by weight.
[0005] Preferably, the solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios comprises, by weight, at least 30-70 parts of calcium-containing solid waste powder, 20-50 parts of solid waste particles, 2-5 parts of reinforcing powder, and 7-23 parts of water.
[0006] As a preferred technical solution, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the calcium-containing solid waste powder is 40-70%, preferably 45-55%.
[0007] As a preferred technical solution, the particle size of the calcium-containing solid waste powder is 0.05-0.15 mm, preferably 0.08-0.1 mm.
[0008] As a preferred technical solution, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the solid waste particles is 20-50%, preferably 30-45%.
[0009] As a preferred technical solution, the particle size of the solid waste particles is ≤6 mm, preferably ≤4.5 mm.
[0010] As a preferred technical solution, the solid waste particles are a combination of solid waste particles 1 with an average particle size ≤ 0.15 mm, solid waste particles 2 with an average particle size of 0.15 mm < ≤ 0.3 mm, solid waste particles 3 with an average particle size of 0.3 mm < ≤ 1.2 mm, solid waste particles 4 with an average particle size of 1.2 mm < ≤ 2.5 mm, and solid waste particles 5 with an average particle size of 2.5 mm < ≤ 4.5 mm.
[0011] As a preferred technical solution, the mass percentages of the solid waste particles 1, solid waste particles 2, solid waste particles 3, solid waste particles 4 and solid waste particles 5 are 0-20%, 10-30%, 15-35%, 10-30% and 10-30% respectively.
[0012] As a preferred technical solution, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the water is 20-40%, preferably 25-35%.
[0013] As a preferred technical solution, the calcium-containing solid waste powder is selected from at least one of steel slag, magnesium slag, calcium silicon slag and carbide slag.
[0014] Preferably, the calcium-containing solid waste powder includes at least steel slag.
[0015] As a preferred technical solution, the solid waste particles are selected from at least one of crude steel slag, crude magnesium slag, marble waste, and granite waste.
[0016] Preferably, the solid waste particles include at least crude steel slag.
[0017] The present invention ensures fine pores, uniform chromaticity and stable performance of the product by controlling the gradation design of solid waste particles in the system.
[0018] As a preferred technical solution, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the reinforcing powder is 2-5%, preferably 2-4%.
[0019] As a preferred technical solution, the raw materials for preparing the reinforcing powder at least include hydrotalcite, isocyanate and a modifier.
[0020] As a preferred technical solution, the hydrotalcite is aluminum-magnesium hydrotalcite.
[0021] As a preferred technical solution, the isocyanate is an isocyanate containing one isocyanate group and / or an isocyanate containing two isocyanate groups.
[0022] Preferably, the isocyanate containing one isocyanate group is selected from at least one of ethyl isocyanate, butyl isocyanate, tert-octyl isocyanate, tetradecyl isocyanate and decyl isocyanate; the isocyanate containing two isocyanate groups is selected from at least one of methylene diisocyanate and isophorone diisocyanate.
[0023] As a preferred technical solution, the isocyanate is an isocyanate containing two isocyanate groups.
[0024] Preferably, the isocyanate is hexamethylene diisocyanate.
[0025] As a preferred technical solution, the modifier is a C10-C25 carboxylate compound.
[0026] Preferably, the modifier is at least one of sodium stearate, calcium stearate and zinc stearate.
[0027] As a preferred technical solution, the mass ratio of the hydrotalcite to the modifier is 1:(0.01-0.05).
[0028] Preferably, the mass ratio of the hydrotalcite to the modifier is 1:(0.02-0.04).
[0029] As a preferred technical solution, the preparation method of the reinforcing powder is as follows: adding hydrotalcite to water and stirring to obtain a slurry, then adding a modifier, stirring at 20-50°C for 10-60 min, centrifuging, washing, and drying to obtain a hydrophobically modified hydrotalcite; taking the hydrophobically modified hydrotalcite and dispersing it in isocyanate, stirring at 50-90°C for 5-24h, filtering, washing, and drying to obtain the reinforcing powder.
[0030] In order to further improve the mechanical strength and waterproof performance of artificial stone, the present invention introduces reinforcing powder made of hydrotalcite, isocyanate, modifier and water into the artificial stone system. On the one hand, from the performance test data of the product, the reinforcing powder can effectively reduce the water absorption rate of artificial stone while improving the flexural strength and compressive strength of artificial stone; on the other hand, the artificial stone can effectively resist the invasion of external acid ions during the later use process, and improve the durability and weather resistance of artificial stone. The inventor analyzed that the reasons may be:
[0031] When the mass ratio of hydrotalcite to modifier is 1:(0.01-0.05), especially 1:(0.02-0.04), the surface of hydrotalcite is coated with a hydrophobic film. The grafted hydrophobic long chain not only improves the water resistance of artificial stone, but also plays a certain protective role for isocyanate inserted into the hydrotalcite interlayer. The reinforcing powder is put into the slurry. In the initial stage of the reaction, the hydrophobic film can prevent the slurry from contacting with isocyanate too early, and prevent isocyanate from releasing carbon dioxide too early. During the mineralization process, as time goes by and the temperature of the system rises, some water molecules will enter the hydrotalcite and react with some isocyanates to generate CO2. Internal carbon dioxide mineralization can be carried out to improve the strength of the product, so as to solve the problem that mineralization usually only occurs on the surface of the product and is difficult to occur inside. In addition, the polymer generated after the isocyanate reaction helps to fill the pores and improve the interface bonding strength. During the later use of the product, due to the erosion of sulfate ions, the artificial stone will expand and produce fine cracks, which may release unreacted isocyanates and react with water in nature to generate healing products, fill the cracks, and improve the durability and weather resistance of the product.
[0032] In addition, hydrotalcite itself can also fill the micro-cracks and pores in the system, improving the density and strength of artificial stone.
[0033] Another aspect of the present invention provides a method for preparing solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios, comprising at least the following steps:
[0034] 1) Mixing calcium-containing solid waste powder, solid waste particles and reinforcing powder to obtain mixed dry material;
[0035] 2) adding water to the mixed dry materials in 1) and stirring evenly to obtain a mixed material;
[0036] 3) putting the mixed material in 2) into a mold and pressing it with a press, the molding pressure is 10-60MPa, the pressure holding time is 1-10 minutes, and after molding, the green body is pushed out by the press to obtain a green body;
[0037] 4) The green body obtained in step 3) is transferred to a curing kiln for moisture-curing, with the humidity in the kiln being 70-95% and the temperature being 40-80°C;
[0038] 5) Pushing the green body of step 4) into a reactor to undergo a mineralization reaction to obtain a plate, the temperature is controlled at 60-120° C., the pressure is controlled at 0.2-0.8 MPa, and the reaction time is 2-10 hours;
[0039] 6) The plate obtained in step 5) is subjected to thickness determination and litchi surface treatment to obtain a surface texture, and then subjected to surface protection treatment to obtain a finished product.
[0040] Preferably, in step 3), the molding pressure is 30-50 MPa and the holding time is 2-4 minutes.
[0041] Preferably, in step 4), the humidity in the kiln is 80-90% and the temperature is 50-70°C.
[0042] Preferably, in step 5), the mineralization reaction temperature is controlled at 80-100° C., the pressure is controlled at 0.5-0.7 MPa, and the reaction time is preferably 6-8 hours.
[0043] Beneficial Effects
[0044] 1. The present invention uses calcium-containing solid waste powder, solid waste particles, reinforcing powder and water to prepare a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. By introducing reinforcing powder, an artificial stone with high mechanical strength and low water absorption is obtained.
[0045] 2. Taking advantage of the interlayer ion exchangeability, adjustable interlayer spacing, and large specific surface area of hydrotalcite, isocyanate is exchanged between layers, and the degree of hydrophobic modification on the surface of hydrotalcite is controlled to adjust the rhythm of isocyanate participating in the system reaction. During the mineralization process, part of the isocyanate reacts with water to generate CO2, which is beneficial to the internal mineralization effect of the product. The product helps to fill the pores, thereby improving the strength of the product; in later use, the invasion of external acid ions causes tiny cracks in the artificial stone, which may cause the isocyanate that has not completely reacted during the mineralization process to react with water in nature to generate healing products to fill the cracks, thereby improving the durability and weather resistance of the product.
[0046] 3. The present invention optimizes the amount of hydrotalcite and modifier in the reinforcing powder and controls the mass ratio of the two to be 1: (0.01-0.05), especially 1: (0.02-0.04), which can effectively balance the relationship between the grafting rate of hydrophobic long chains on the hydrotalcite and the degree of intercalation of isocyanate into the hydrotalcite, and exert the protective effect of the hydrophobic film on the hydrotalcite on the intercalated isocyanate, thereby controlling the reaction rate of the isocyanate in the system to regulate the performance of the artificial stone. DETAILED DESCRIPTION
[0047] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0048] Example
[0049] The solid waste-based carbon mineralized artificial stone of the present invention is suitable for high pressure resistance scenarios. The raw materials for its preparation include at least 30-80 parts of calcium-containing solid waste powder, 20-70 parts of solid waste particles, 1-8 parts of reinforcing powder, and 5-50 parts of water, calculated by weight.
[0050] A method for preparing solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios comprises at least the following steps:
[0051] 1) Mixing calcium-containing solid waste powder, solid waste particles and reinforcing powder to obtain mixed dry material;
[0052] 2) adding water to the mixed dry materials in 1) and stirring evenly to obtain a mixed material;
[0053] 3) putting the mixed material in 2) into a mold and pressing it with a press, the molding pressure is 10-60MPa, the pressure holding time is 1-10 minutes, and after molding, the green body is pushed out by the press to obtain a green body;
[0054] 4) The green body obtained in step 3) is transferred to a curing kiln for moisture-curing, with the humidity in the kiln being 70-95% and the temperature being 40-80°C;
[0055] 5) Pushing the green body of step 4) into a reactor to undergo a mineralization reaction to obtain a plate, the temperature is controlled at 60-120° C., the pressure is controlled at 0.2-0.8 MPa, and the reaction time is 2-10 hours;
[0056] 6) The plate obtained in step 5) is subjected to thickness determination and litchi surface treatment to obtain a surface texture, and then subjected to surface protection treatment to obtain a finished product.
[0057] In some embodiments, the solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios comprises, by weight, at least 30-70 parts of calcium-containing solid waste powder, 20-50 parts of solid waste particles, 2-5 parts of reinforcing powder, and 7-23 parts of water.
[0058] In some embodiments, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the calcium-containing solid waste powder is 40-70%, preferably 45-55%.
[0059] In some embodiments, the particle size of the calcium-containing solid waste powder is 0.05-0.15 mm.
[0060] In some embodiments, the particle size of the calcium-containing solid waste powder is 0.08-0.1 mm.
[0061] In some embodiments, the mass of the solid waste particles accounts for 20-50% of the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios.
[0062] In some embodiments, based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios, the mass proportion of the solid waste particles is 30-45%.
[0063] In some embodiments, the particle size of the solid waste particles is ≤6 mm.
[0064] In some embodiments, the particle size of the solid waste particles is ≤4.5 mm.
[0065] In some embodiments, the solid waste particles are a combination of solid waste particles 1 with an average particle size ≤ 0.15 mm, solid waste particles 2 with an average particle size of 0.15 mm < ≤ 0.3 mm, solid waste particles 3 with an average particle size of 0.3 mm < ≤ 1.2 mm, solid waste particles 4 with an average particle size of 1.2 mm < ≤ 2.5 mm, and solid waste particles 5 with an average particle size of 2.5 mm < ≤ 4.5 mm.
[0066] In some embodiments, the mass percentages of the solid waste particles 1, solid waste particles 2, solid waste particles 3, solid waste particles 4 and solid waste particles 5 are 0-20%, 10-30%, 15-35%, 10-30% and 10-30% respectively.
[0067] In some embodiments, the mass proportion of the water is 20-40% based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios.
[0068] In some embodiments, the mass proportion of water is 25-35% based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios.
[0069] In some embodiments, the calcium-containing solid waste powder is selected from at least one of steel slag, magnesium slag, calcium-silicon slag, and carbide slag.
[0070] In some embodiments, the calcium-containing solid waste powder includes at least steel slag.
[0071] In some embodiments, the solid waste particles are selected from at least one of crude steel slag, crude magnesium slag, marble waste, and granite waste.
[0072] In some embodiments, the solid waste particles include at least crude steel slag.
[0073] The present invention ensures fine pores, uniform chromaticity and stable performance of the product by controlling the gradation design of solid waste particles in the system.
[0074] In some embodiments, the mass proportion of the reinforcing powder is 2-5% based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw materials suitable for high pressure resistance scenarios.
[0075] In some embodiments, the mass proportion of the reinforcing powder is 2-4% based on the total weight of the solid waste-based carbon mineralized artificial stone preparation raw material suitable for high pressure resistance scenarios.
[0076] In some embodiments, the raw materials for preparing the reinforcing powder include at least hydrotalcite, isocyanate and a modifier.
[0077] In some embodiments, the hydrotalcite is aluminum-magnesium hydrotalcite.
[0078] In some embodiments, the isocyanate is an isocyanate containing one isocyanate group and / or an isocyanate containing two isocyanate groups.
[0079] In some embodiments, the isocyanate containing one isocyanate group is selected from at least one of ethyl isocyanate, butyl isocyanate, tert-octyl isocyanate, tetradecyl isocyanate, and decyl isocyanate; the isocyanate containing two isocyanate groups is selected from at least one of methylene diisocyanate and isophorone diisocyanate.
[0080] In some embodiments, the isocyanate is an isocyanate containing 2 isocyanate groups.
[0081] In some embodiments, the isocyanate is hexamethylene diisocyanate.
[0082] In some embodiments, the modifier is a C10-C25 carboxylate compound.
[0083] In some embodiments, the modifier is at least one of sodium stearate, calcium stearate, and zinc stearate.
[0084] In some embodiments, the mass ratio of the hydrotalcite to the modifier is 1:(0.01-0.05).
[0085] In some embodiments, the mass ratio of the hydrotalcite to the modifier is 1:(0.02-0.04).
[0086] In some embodiments, the preparation method of the reinforcing powder is as follows: adding hydrotalcite to water and stirring to obtain a slurry, then adding a modifier, stirring at 20-50°C for 10-60 min, centrifuging, washing, and drying to obtain a hydrophobically modified hydrotalcite; taking the hydrophobically modified hydrotalcite and dispersing it in isocyanate, stirring at 50-90°C for 5-24h, filtering, washing, and drying to obtain the reinforcing powder.
[0087] In order to further improve the mechanical strength and waterproof performance of artificial stone, the present invention introduces reinforcing powder made of hydrotalcite, isocyanate, modifier and water into the artificial stone system. On the one hand, from the performance test data of the product, the reinforcing powder can effectively reduce the water absorption rate of artificial stone while improving the flexural strength and compressive strength of artificial stone; on the other hand, the artificial stone can effectively resist the invasion of external acid ions during the later use process, and improve the durability and weather resistance of artificial stone. The inventor analyzed that the reasons may be:
[0088] When the mass ratio of hydrotalcite to modifier is 1:(0.01-0.05), especially 1:(0.02-0.04), the surface of hydrotalcite is coated with a hydrophobic film. The grafted hydrophobic long chain not only improves the water resistance of artificial stone, but also plays a certain protective role for isocyanate inserted into the hydrotalcite interlayer. The reinforcing powder is put into the slurry. In the initial stage of the reaction, the hydrophobic film can prevent the slurry from contacting with isocyanate too early, and prevent isocyanate from releasing carbon dioxide too early. During the mineralization process, as time goes by and the temperature of the system rises, some water molecules will enter the hydrotalcite and react with some isocyanates to generate CO2. Internal carbon dioxide mineralization can be carried out to improve the strength of the product, so as to solve the problem that mineralization usually only occurs on the surface of the product and is difficult to occur inside. In addition, the polymer generated after the isocyanate reaction helps to fill the pores and improve the interface bonding strength. During the later use of the product, due to the erosion of sulfate ions, the artificial stone will expand and produce fine cracks, which may release unreacted isocyanates and react with water in nature to generate healing products, fill the cracks, and improve the durability and weather resistance of the product.
[0089] In addition, hydrotalcite itself can also fill the micro-cracks and pores in the system, improving the density and strength of artificial stone.
[0090] In some embodiments, in step 3), the molding pressure is 30-50 MPa, and the holding time is 2-4 minutes.
[0091] In some embodiments, in step 4), the humidity in the kiln is 80-90% and the temperature is 50-70°C.
[0092] In some embodiments, in step 5), the mineralization reaction temperature is controlled at 80-100° C., the pressure is controlled at 0.5-0.7 MPa, and the reaction time is preferably 6-8 hours.
[0093] The artificial stone prepared according to the above scheme has higher mechanical strength and lower water absorption rate.
[0094] Example 1
[0095] The present embodiment provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. The raw materials for preparing the artificial stone are, by weight: 50 parts by weight of calcium-containing solid waste powder, 33 parts by weight of solid waste particles, 3.3 parts by weight of reinforcing powder and 15 parts by weight of water.
[0096] The calcium-containing solid waste powder is steel slag, and its average particle size is 0.09 mm.
[0097] The solid waste particles are a mixed powder of 26.5 parts by weight of crude steel slag and 6.5 parts by weight of marble waste. The gradation design is as follows, calculated by weight: 4.95 parts by weight of solid waste particles 1, with an average particle size of 0.08 mm, 6.6 parts by weight of solid waste particles 2, with an average particle size of 0.25 mm, 8.25 parts by weight of solid waste particles 3, with an average particle size of 0.82 mm, 6.6 parts by weight of solid waste particles 4, with an average particle size of 2 mm, and 6.6 parts by weight of solid waste particles 5, with an average particle size of 3.3 mm.
[0098] The raw materials for preparing the reinforcing powder are: aluminum-magnesium hydrotalcite, sodium stearate, hexamethylene diisocyanate and water.
[0099] The preparation method of the reinforcing powder is as follows: 20 parts by weight of magnesium aluminum hydrotalcite is added to 70 parts by weight of water, stirred into slurry, and then 0.5 parts by weight of sodium stearate is added, stirred at 35°C for 40 minutes, centrifuged, washed, and dried at 60°C for 15 hours to obtain hydrophobically modified hydrotalcite; the obtained hydrophobically modified hydrotalcite is placed in excess isocyanate, stirred at 75°C for 8 hours, filtered, washed with n-hexane three times, and then dried at 65°C for 15 hours to obtain reinforcing powder.
[0100] The method for preparing the solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios comprises the following steps:
[0101] 1) Mixing calcium-containing solid waste powder, solid waste particles and reinforcing powder to obtain mixed dry material;
[0102] 2) adding water to the mixed dry materials in 1) and stirring evenly to obtain a mixed material;
[0103] 3) putting the mixed material in 2) into a mold and pressing it with a press, with a molding pressure of 40 MPa and a holding time of 3 minutes, and after molding, pushing out the green body with a press;
[0104] 4) The green body obtained in step 3) is transferred to a curing kiln for moisture-maintaining curing, with the humidity in the kiln being 90% and the temperature being 60°C;
[0105] 5) pushing the green body of step 4) into a reactor to undergo a mineralization reaction to obtain a plate, with the temperature controlled at 90° C., the pressure controlled at 0.6 MPa, and the reaction time being 7 h;
[0106] 6) The plate obtained in step 5) is subjected to thickness determination and litchi surface treatment to obtain a surface texture, and then subjected to surface protection treatment to obtain a finished product.
[0107] Example 2
[0108] The present embodiment provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. The raw materials for preparing the artificial stone are, by weight: 30 parts by weight of calcium-containing solid waste powder, 20 parts by weight of solid waste particles, 2 parts by weight of reinforcing powder and 9 parts by weight of water.
[0109] The calcium-containing solid waste powder is steel slag, and its average particle size is 0.08 mm.
[0110] The solid waste particles are a mixed powder of 16 parts by weight of crude steel slag and 4 parts by weight of marble waste. The gradation design is as follows, calculated by weight: 3 parts by weight of solid waste particles 1, with an average particle size of 0.03 mm, 4 parts by weight of solid waste particles 2, with an average particle size of 0.16 mm, 5 parts by weight of solid waste particles 3, with an average particle size of 0.32 mm, 4 parts by weight of solid waste particles 4, with an average particle size of 1.21 mm, and 4 parts by weight of solid waste particles 5, with an average particle size of 2.6 mm.
[0111] The raw materials for preparing the reinforcing powder are: aluminum-magnesium hydrotalcite, sodium stearate, hexamethylene diisocyanate and water.
[0112] The preparation method of the reinforcing powder is as follows: 10 parts by weight of magnesium aluminum hydrotalcite is added to 60 parts by weight of water, stirred into slurry, and then 0.2 parts by weight of sodium stearate is added, stirred at 35°C for 40 minutes, centrifuged, washed, and dried at 60°C for 15 hours to obtain hydrophobically modified hydrotalcite; the obtained hydrophobically modified hydrotalcite is placed in excess isocyanate, stirred at 75°C for 8 hours, filtered, washed with n-hexane three times, and then dried at 65°C for 15 hours to obtain reinforcing powder.
[0113] The preparation method of artificial stone is the same as that of Example 1.
[0114] Example 3
[0115] The present embodiment provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios. The raw materials for preparing the artificial stone are, by weight: 70 parts by weight of calcium-containing solid waste powder, 46 parts by weight of solid waste particles, 5 parts by weight of reinforcing powder and 21 parts by weight of water.
[0116] The calcium-containing solid waste powder is steel slag, and its average particle size is 0.1 mm.
[0117] The solid waste particles are a mixed powder of 37 parts by weight of crude steel slag and 9 parts by weight of marble waste. The gradation design is as follows, calculated by weight: 6.3 parts by weight of solid waste particles 1, with an average particle size of 0.15 mm, 8.2 parts by weight of solid waste particles 2, with an average particle size of 0.3 mm, 10.5 parts by weight of solid waste particles 3, with an average particle size of 1.18 mm, 8.2 parts by weight of solid waste particles 4, with an average particle size of 2.5 mm, and 12.8 parts by weight of solid waste particles 5, with an average particle size of 4.5 mm.
[0118] The raw materials for preparing the reinforcing powder are: aluminum-magnesium hydrotalcite, sodium stearate, hexamethylene diisocyanate and water.
[0119] The preparation method of the reinforcing powder is as follows: 30 parts by weight of magnesium aluminum hydrotalcite is added to 85 parts by weight of water, stirred into slurry, then 0.9 parts by weight of sodium stearate is added, stirred at 35°C for 40 minutes, centrifuged, washed, and dried at 60°C for 15 hours to obtain hydrophobically modified hydrotalcite; the obtained hydrophobically modified hydrotalcite is placed in excess isocyanate, stirred at 75°C for 8 hours, filtered, washed with n-hexane three times, and then dried at 65°C for 15 hours to obtain reinforcing powder.
[0120] The preparation method of artificial stone is the same as that of Example 1.
[0121] Example 4
[0122] This embodiment provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios, which is different from Example 1 in that, in terms of weight parts, the amount of aluminum-magnesium hydrotalcite used in the preparation of the reinforcing powder is 20 parts by weight, and the amount of sodium stearate used is 0.2 parts by weight.
[0123] Example 5
[0124] This embodiment provides a solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios, which is different from Example 1 in that, in terms of weight parts, the amount of aluminum-magnesium hydrotalcite used in the preparation of the reinforcing powder is 20 parts by weight, and the amount of sodium stearate used is 1.0 part by weight.
[0125] Example 6
[0126] This comparative example provides an artificial stone, which is different from Example 1 in that hexamethylene diisocyanate in the preparation of the reinforcing powder is replaced by isophorone diisocyanate.
[0127] Comparative Example 1
[0128] This comparative example provides an artificial stone, which is different from Example 1 in that no reinforcing powder is used.
[0129] Comparative Example 2
[0130] This comparative example provides an artificial stone, which is different from Example 1 in that sodium stearate in the preparation process of the reinforcing powder is replaced by sodium acetate.
[0131] Performance Testing
[0132] With reference to JC / T2604-2021 "Stone-like concrete panels and tiles", the flexural strength and compressive strength tests were conducted on the artificial stones obtained in each embodiment and comparative example. With reference to GB / T4111-2013 "Test methods for concrete blocks and bricks", the water absorption rate of the artificial stones obtained in each embodiment and comparative example was tested.
[0133] The test results are shown in Table 1:
[0134] Table 1
[0135]
[0136] The data in Table 1 show that:
[0137] The flexural strength of the artificial stone prepared in Examples 1-6 reached above 17.17 MPa, the compressive strength reached above 127.25 MPa, and the water absorption rate was lower than 2.0%, with excellent performance.
[0138] Compared with Example 1, the mechanical properties and water absorption rate of Example 4 are worse. This may be due to the fact that there is less sodium stearate in the preparation process of the reinforcing powder, which deteriorates the hydrophobic modification effect on the hydrotalcite. Water can easily invade the reinforcing powder core, causing the intercalated hexamethylene diisocyanate to undergo polymerization reaction and produce CO2 in advance, which not only destroys the pore structure of the green body, but also causes the mineralization effect to deteriorate. Therefore, the mechanical strength and waterproof effect of the product are both deteriorated.
[0139] Compared with Example 1, the compressive strength and flexural strength of Example 5 are both reduced. The reason may be that: there is more sodium stearate, and a dense film is formed on the surface of the hydrotalcite. The long hydrophobic chains are entangled with each other, and the wrapping is strong, which is not conducive to the subsequent intercalation behavior of hexamethylene diisocyanate. The intercalated isocyanate is less, the generated organic skeleton structure becomes less, and the internal synergistic strengthening mineralization effect is significantly weakened. The strength of the product inside and outside is uneven, so the mechanical properties of the product are deteriorated.
[0140] The mechanical strength of Example 6 is reduced compared with Example 1, which may be due to the relatively large steric hindrance of the isophorone diisocyanate structure and the relatively small amount of intercalation into the modified hydrotalcite, so the mechanical strength of the product is reduced.
[0141] Comparative Example 1 Compared with Example 1, without adding reinforcing powder, the mechanical strength and waterproofness of the product are both deteriorated.
[0142] Compared with Example 1, the mechanical properties and water absorption rate of the product of Comparative Example 2 are significantly reduced. The reason may be that the carboxylate in sodium acetate undergoes ion exchange with the anion in the hydrotalcite, forming a competitive relationship with the isocyanate, and there is no hydrophobic long chain to protect the isocyanate. After the reinforcing powder is added to the system, the isocyanate is quickly released, so the performance of the product is reduced.
Claims
1. A solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios, characterized in that: The raw materials for its preparation include at least 30-80 parts by weight of calcium-containing solid waste powder, 20-70 parts of solid waste particles, 1-8 parts of reinforcing powder, and 5-50 parts of water. The raw materials for the preparation of the reinforcing powder include at least hydrotalcite, isocyanate and a modifier; the mass ratio of the hydrotalcite to the modifier is 1:(0.01-0.05); the modifier is at least one of sodium stearate, calcium stearate and zinc stearate.
2. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The mass ratio of the hydrotalcite to the modifier is 1:(0.02-0.04).
3. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The isocyanate is an isocyanate containing one isocyanate group and / or an isocyanate containing two isocyanate groups; The isocyanate containing one isocyanate group is selected from at least one of ethyl isocyanate, butyl isocyanate, tert-octyl isocyanate, tetradecyl isocyanate, and decyl isocyanate; The isocyanate containing two isocyanate groups is selected from at least one of methylene diisocyanate and isophorone diisocyanate.
4. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The isocyanate is an isocyanate containing two isocyanate groups.
5. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The isocyanate is hexamethylene diisocyanate.
6. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The preparation method of the reinforcing powder is as follows: adding hydrotalcite into water and stirring to obtain slurry, then adding a modifier, stirring at 20-50° C. for 10-60 min, centrifuging, washing, and drying to obtain hydrophobically modified hydrotalcite; The hydrophobically modified hydrotalcite is dispersed in isocyanate, stirred at 50-90° C. for 5-24 hours, filtered, washed and dried to obtain the product.
7. The solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to claim 1, characterized in that: The solid waste particles are selected from solid waste particles 1 with an average particle size ≤ 0.15mm, solid waste particles 2 with an average particle size of 0.15mm < ≤ 0.3mm, solid waste particles 3 with an average particle size of 0.3mm < ≤ 1.2mm, solid waste particles 4 with an average particle size of 1.2mm < ≤ 2.5mm and solid waste particles 5 with an average particle size of 2.5mm < ≤ 4.5mm; the mass percentages of the solid waste particles 1, solid waste particles 2, solid waste particles 3, solid waste particles 4 and solid waste particles 5 are 0-20%, 10-30%, 15-35%, 10-30% and 10-30% respectively.
8. A method for preparing solid waste-based carbon mineralized artificial stone suitable for high pressure resistance scenarios according to any one of claims 1 to 7, characterized in that: At least the following steps are included: 1) mixing calcium-containing solid waste powder, solid waste particles and reinforcing powder to obtain a mixed dry material; 2) adding water to the mixed dry materials in step 1) and stirring evenly to obtain a mixed material; 3) putting the mixed material in step 2) into a mold and pressing it with a press, the molding pressure is 10-60 MPa, the pressure holding time is 1-10 minutes, and after molding, the green body is pushed out by the press to obtain a green body; 4) transferring the green body obtained in step 3) to a curing kiln for moisture-curing, wherein the humidity in the kiln is 70-95% and the temperature is 40-80° C.; 5) pushing the green body of step 4) into a reactor to carry out a mineralization reaction to obtain a plate, the temperature is controlled at 60-120° C., the pressure is controlled at 0.2-0.8 MPa, and the reaction time is 2-10 h; 6) The plate obtained after the reaction in step 5) is subjected to thickness determination and litchi surface treatment to obtain surface texture, and then subjected to surface protection treatment to obtain a finished product.