A whole core flame retardant conveyor belt covering rubber for coal mines and preparation method thereof

By using montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material as a flame retardant, the problem of large amounts of flame retardants used in coal mine conveyor belts and poor effects is solved, and good flame retardancy is achieved. The combination of effect and tensile performance improves the overall performance and production efficiency of the conveyor belt.

CN118496592BActive Publication Date: 2024-10-15XIAN ZHONGZHUANG WEINAN RUBBER PROD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410946827.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing coal mine conveyor belts use a large amount of flame retardants, resulting in poor flame retardant effects and affecting the tensile properties of the conveyor belts.

Method used

Montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is used as the flame retardant. Through the joint action of its layered network structure and magnesium particles, the flame retardant performance of the conveyor belt is enhanced while reducing the flame retardant. amount of usage.

Benefits of technology

It achieves good flame retardant effect while maintaining the softness and toughness of the conveyor belt, extending its service life, simplifying the production process and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a whole-core flame-retardant conveyor belt covering rubber for coal mines and a preparation method thereof, which belongs to the technical field of flame-retardant conveyor belts for mines, and comprises the following raw materials: styrene-butadiene rubber, EPDM rubber, EPDM rubber, reinforcing agent, plasticizer, softener and flame retardant, wherein the flame retardant is a montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material. The technical solution provided by the present invention realizes the purpose of using less flame retardant, having good flame retardant effect and not affecting the tensile performance of the conveyor belt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame-retardant conveyor belts for mines, and in particular to a covering rubber for a whole-core flame-retardant conveyor belt for coal mines and a preparation method thereof. Background Art

[0002] In recent years, with the improvement of coal mine production capacity and the continuous advancement of working faces, the underground transportation distance and task volume of mines have become larger and larger, and the requirements for conveyor belts have gradually increased. The conveyor belt is the most powerful and widely used transportation device in underground production and transportation of coal mines. It is often in an overloaded operation state in coal mines. The mine environment is special. The air contains a lot of flammable and explosive substances such as gas and coal powder. Coal itself is also a flammable substance. If the conveyor belt produces sparks due to various reasons, it is very easy to cause fire and other safety accidents. Therefore, the flame retardant properties of conveyor belts for coal mines are particularly important.

[0003] In order to improve the flame retardant properties of conveyor belts for coal mines, the patent with publication number CN105254961A and patent name "A kind of anti-cutting flame retardant conveyor belt covering rubber for coal mines and its preparation method" discloses a method for preparing anti-cutting flame retardant conveyor belt covering rubber for coal mines, which not only meets the flame retardant performance requirements of MT668 flame retardant conveyor belt for coal mines, but also has anti-cutting performance. However, the covering rubber in the above technical scheme includes 60-80 parts of chloroprene rubber, 20-40 parts of butadiene rubber, 45-75 parts of reinforcing filler, 1-5 parts of processing aid, 0.2-5 parts of vulcanizer, 0.8-7 parts of vulcanization accelerator, 4-12 parts of vulcanization activator, 5-25 parts of plasticizer, 1-3 parts of antioxidant and 30-60 parts of flame retardant. After plasticizing and mixing, the anti-cutting flame-retardant conveyor belt covering rubber for coal mine is obtained, wherein the number of flame retardants is large. A large increase in the number of flame retardants will reduce the toughness of the conveyor belt, affect the tensile properties of the rubber itself, and have poor flame retardant effect in actual application.

[0004] Therefore, it is necessary to provide a whole-core flame-retardant conveyor belt covering rubber and a preparation method for coal mines, which can achieve good flame retardant effect with a small amount of flame retardant, thereby solving the current problem of large amount of flame retardant used, poor effect and affecting the tensile performance of the conveyor belt. Summary of the invention

[0005] In view of this, the present invention provides a whole-core flame-retardant conveyor belt covering rubber for coal mines and a preparation method thereof, which achieves the purpose of using less flame retardant and having good flame retardant effect without affecting the tensile performance of the conveyor belt.

[0006] To achieve the above-mentioned purpose, the present invention provides a whole-core flame-retardant conveyor belt covering rubber for coal mines, comprising the following raw materials: styrene-butadiene rubber, EPDM rubber, EPDM rubber, a reinforcing agent, a plasticizer, a softener and a flame retardant, wherein the flame retardant is a montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material.

[0007] The whole-core flame-retardant conveyor belt covering rubber for coal mines provided by the present invention uses raw materials including montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite materials. The layered network structure of montmorillonite can prevent the spread of flammable components and the entry of oxygen. At the same time, after combustion, the small molecular silicate structure inside the montmorillonite is disintegrated, and a clay carbon layer can be formed to prevent combustion. The magnesium-containing microparticle structure is decomposed by heat to form active MgO, which is easy to absorb free radicals and carbon, and delay the ignition of the material. When the montmorillonite network structure is disintegrated by heat, the active MgO can capture free radicals from the interlayer gaps, prevent the combustion reaction from occurring, and protect the composite structure from further destruction. The exposed magnesium-containing microsphere structure can also exert its flame retardant effect. The two work together to enhance the flame retardant ability of the conveyor belt material.

[0008] The montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material has a strong flame retardant effect. While achieving excellent flame retardant effect, it reduces the use of flame retardants and avoids the influence of large amounts of flame retardants on the softness and toughness of the conveyor belt. It maintains the good performance of the conveyor belt cover rubber at the bends and increases its service life.

[0009] Optionally, the montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is prepared by the following steps:

[0010] S1, using montmorillonite and bis(hydroxydodecyltrimethylammonium chloride) to swell to obtain a swollen montmorillonite structure, then adding sodium alginate solution dropwise, stirring, solid-liquid separation, and grinding to obtain montmorillonite powder;

[0011] S2, using sodium dodecylbenzene sulfonate anionic surfactant, hydroxy calcium phosphate and styrene mixed with mixed acid and reacted, then adding initiator azobisisobutyl cyanide to initiate polymerization reaction to obtain solution A; dissolving MgCl2 to prepare a mixed solution, and the obtained solution is recorded as solution B; taking solution A, adding chloroform and solution B to obtain a suspension of nitro polystyrene microspheres coated with hydrated magnesium chloride;

[0012] S3, adding the montmorillonite powder obtained in step S1, dropping the sodium sulfite solution, stirring, removing the solvent, drying, and grinding to obtain a montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material.

[0013] The montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material provided by the present invention is that the interlayer spacing of the montmorillonite is opened after being treated with dihydroxy dodecyl trimethyl ammonium chloride, the hydrogen bond structure between adjacent layers is weakened, and then the montmorillonite is peeled off after being treated with alginate anion groups and interlayer repulsion. Nitropolystyrene-hydrated magnesium chloride microspheres are added and mixed, and the microspheres are interspersed between the layers. At this time, the structure is not fixed and unstable. After the sulfite anion is introduced into the system, SO3 2-One end undergoes sulfonation substitution reaction with the benzene ring and connects to the microsphere, while the SO3 introduced 2- Ions can form hydrogen bonds with montmorillonite silicates through SO3 2- The bonding effect maintains the stability of the relative position of montmorillonite and sulfonated nitropolystyrene-hydrated magnesium chloride microspheres, thereby constructing a relatively stable connection structure to ensure the stability of the flame retardant. At the same time, the combined effect of montmorillonite and hydrated magnesium chloride enhances the flame retardant ability of the conveyor belt.

[0014] Optionally, during the swelling in S1, ethanol and water are further added for heating and stirring, the mass ratio of ethanol to water is 1:1, the heating temperature is 75-80°C, the stirring time is 1.5-2.5h, the stirring rate is 240-260r / min, and the mass fraction of the sodium alginate solution is 1-2%.

[0015] The present invention uses 1-2% sodium alginate solution to fully destroy the hydrogen bond structure between montmorillonite layers, and can obtain exfoliated montmorillonite powder.

[0016] Optionally, the reaction conditions after mixing in S2 include a temperature of 45-50°C, a stirring rate of 240-260 r / min, and a stirring time of 1.5-2.5 h; the conditions during the polymerization reaction include a temperature of 85-90°C, a stirring rate of 70-80 r / min, and a stirring time of 2-2.5 h.

[0017] The stirring rates used in the present invention are different, and are divided into high-speed stirring and low-speed stirring. The dispersion state and reaction conditions required in each step can be achieved through different stirring rates.

[0018] Optionally, the mass fraction of the solute in the mixed solution in S2 is 4-6%, the mixed acid is sulfuric acid and nitric acid, and the mass ratio of sulfuric acid to nitric acid is 3:2.

[0019] Optionally, after adding montmorillonite powder to S3, ultrasonic dispersion is adopted, the ultrasonic dispersion time is 20-30 min, and the ultrasonic dispersion temperature is 50-65° C.; when adding sodium sulfite solution, the low-speed stirring time is 1-2 h, and the stirring rate is 70-80 r / min.

[0020] In the present invention, ultrasonic dispersion is used to form a uniform dispersion structure between the suspension microspheres and the montmorillonite. After the sodium sulfite solution is added, low-speed stirring is performed to form a connection structure between the microspheres and the montmorillonite dispersion structure due to hybridization, thereby forming a solidified structure.

[0021] Optionally, it also includes a vulcanizer, a catalyst, an accelerator and an antioxidant, and the weight proportions of each raw material are 15-20 parts of styrene-butadiene rubber, 60-70 parts of EPDM rubber, 25-30 parts of EPDM rubber, 40-45 parts of a reinforcing agent, 10-15 parts of a plasticizer, 5-10 parts of a vulcanizer, 1.5-2 parts of a catalyst, 5-7 parts of an accelerator, 2-3 parts of an antioxidant, 5-10 parts of a softener, and 8-10 parts of a flame retardant.

[0022] Optionally, the reinforcing agent is carbon black N234; the plasticizer is stearate; the vulcanizing agent is 1,1-bis(tert-butyl)-3,3,5-trimethylcyclohexane; the catalyst is trimethylenediamine; the accelerator is zinc oxide; and the softener is paraffin oil.

[0023] In order to achieve the above object, the present invention also provides a method for preparing the above-mentioned whole-core flame-retardant conveyor belt covering rubber for coal mines, comprising the following steps:

[0024] Step 1, plasticizing: weighing styrene-butadiene rubber, EPDM rubber, EPDM rubber and plasticizer according to weight proportions, putting them into an internal mixer, and plasticizing to obtain a mixed rubber product;

[0025] Step 2, mixing: putting the accelerator, antioxidant, softener, reinforcing agent and montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material into the plasticizing rubber system, repeatedly returning the glue after the glue is discharged to make the components evenly mixed, and then standing and cooling to make the mixed rubber sheet cool and set;

[0026] Step 3: Vulcanization: Put the film product in step 2 into an internal mixer, add a vulcanizing agent and a catalyst into the system, control the reaction time and temperature, repeatedly return the glue after debinding, mix all the components evenly, and obtain a covering rubber film.

[0027] In the present invention, the raw materials are plasticized, mixed and vulcanized to obtain a covering rubber film. A small amount of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material powder is added during the mixing process, and the viscosity and stickiness during the mixing process can also be reduced, thereby simplifying the production process and improving the production efficiency.

[0028] Optionally, the plasticizing temperature is controlled at 150-160°C, the mixing and debonding temperature range is 125-135°C; the vulcanization debonding temperature is 95-100°C; and the thickness of the covering rubber film is 6-7mm.

[0029] The above technical solution of the present invention includes at least the following beneficial effects:

[0030] The present invention provides a whole-core flame-retardant conveyor belt covering rubber for coal mines. The flame-retardant conveyor belt covering rubber is composed of a flame retardant montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material and various rubber components, reinforcing agents, plasticizers and other ingredients. The flame retardant effect is ensured while reducing the amount of flame retardant used, avoiding affecting the softness and toughness of the conveyor belt. The layered network structure of montmorillonite in the montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material prevents the spread of flammable components, thereby achieving a flame retardant effect.

[0031] The montmorillonite layered structure disintegrates when heated, and the magnesium-containing microparticle structure is also decomposed into active MgO, capturing free radicals and carbon in the interlayer gaps, preventing the combustion reaction, delaying the ignition of the material, and achieving a flame retardant effect; the small molecule silicate structure inside the montmorillonite disintegrates after combustion to form a clay charcoal layer, which prevents combustion and achieves a flame retardant effect. Through layered flame retardancy, the flame retardant effect of the conveyor belt is improved.

[0032] The invention provides a method for preparing a whole-core flame-retardant conveyor belt covering rubber for coal mines, which reduces the use of flame retardants, reduces the viscosity and stickiness during the mixing process, and improves production efficiency. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0034] Example 1

[0035] The conveyor belt covering rubber provided by the present invention comprises the following raw materials in parts by weight: 20 parts of styrene-butadiene rubber, 60 parts of ethylene-propylene-diene rubber, 25 parts of ethylene-propylene-diene rubber, 45 parts of reinforcing agent, 15 parts of plasticizer, 5 parts of vulcanizing agent, 2 parts of catalyst, 7 parts of accelerator, 3 parts of antioxidant, 10 parts of softener and 10 parts of flame retardant, wherein the flame retardant is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres.

[0036] The method for preparing the conveyor belt covering rubber provided by the present invention comprises the following steps:

[0037] Step 1, plasticizing: taking styrene-butadiene rubber, EPDM rubber, EPDM rubber and plasticizer stearate, putting them into an internal mixer, controlling the temperature at 160°C, and plasticizing to obtain a mixed rubber product;

[0038] Step 2, mixing: putting the accelerator zinc oxide, antioxidant, softener paraffin oil, reinforcing agent carbon black N234 and flame retardant montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material into the plasticizing rubber system, controlling the temperature and pressure of the reaction system, starting to discharge the glue at 125°C, repeatedly returning the glue after discharge, so that the components are evenly mixed, and then standing to cool, so that the mixed rubber sheet is cooled and shaped;

[0039] Step 3, vulcanization: put the film product in step 2 into the internal mixer, add the vulcanizing agent 1,1-bis(tert-butyl)-3,3,5-trimethylcyclohexane and the catalyst trimethylenediamine into the system, control the reaction time and system pressure, start the glue discharge when the temperature is maintained at 100°C, repeat the glue return operation to mix the components evenly. Control the film thickness to 7mm and the film width to 600mm, and store it after cooling to 35°C.

[0040] The flame retardant used in the embodiment of the present invention is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres, and the preparation method comprises the following steps:

[0041] 1) Weigh 2.1g of montmorillonite and 0.8g of dihydroxydodecyltrimethylammonium chloride, add them into a 500ml three-necked flask, add 120ml of ethanol / water (mass ratio is 1 / 1) mixed dispersant, heat to 80℃, stir at 260r / min for 1.5h to obtain a swollen montmorillonite structure, then slowly drop 10ml of 2% sodium alginate solution into the solution, adjust the solution pH, control the speed at 240r / min, fully destroy the hydrogen bond structure between montmorillonite layers, then separate the solid and liquid, wash, dry in vacuum at 90℃, and grind to obtain exfoliated montmorillonite powder.

[0042] 2) 1.2 g of sodium dodecylbenzene sulfonate anionic surfactant, 0.6 g of calcium hydroxyphosphate, and 2.3 g of styrene were added to a reactor, nitrogen was introduced into the system to exhaust the air, and a mixed acid of sulfuric acid and nitric acid in a ratio of 3:2 was added at 50°C with high-speed stirring. After reacting for 2 h, 0.02 g of initiator azobisisobutyl cyanide was added to the system, the magnetic stirring speed was controlled to 70 r / min, and polymerization was initiated at 90°C for 2.5 h to obtain a nitropolystyrene microsphere solution grafted with anionic surfactant, which was recorded as solution A.

[0043] 3) Prepare MgCl2 for dissolution, adjust the pH of the solution with anhydrous ethanol and 0.5% hydrochloric acid solution, and prepare a mixed solution with a mass fraction of 6%. The resulting solution is recorded as solution B.

[0044] 4) Take 5 ml of solution A in a flask, add 30 ml of chloroform to disperse it, add the treated solution B to the solution A dispersed with chloroform, stir thoroughly to obtain a suspension of nitropolystyrene microspheres coated with hydrated magnesium chloride.

[0045] 5) Then the powder obtained in 1) is put into the suspension system, chloroform is added to fully disperse it, the temperature is controlled at 65°C, and ultrasonication is performed for 30 minutes to allow the suspension microspheres and montmorillonite to form a uniform dispersion structure. Then 1% sodium sulfite solution is slowly added to the system, the temperature is controlled to maintain at 60°C, and stirring is performed at a low speed of 80r / min. After the reaction is allowed to stand for 1 hour, the microparticles and montmorillonite dispersion structure are solidified due to hybridization. The solvent is removed, the mixture is dried, and the powder of the dispersion structure of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is obtained by grinding.

[0046] Example 2

[0047] The conveyor belt covering rubber provided by the present invention comprises the following raw materials in parts by weight: 15 parts of styrene-butadiene rubber, 70 parts of ethylene-propylene-diene rubber, 30 parts of ethylene-propylene-diene rubber, 40 parts of reinforcing agent, 10 parts of plasticizer, 10 parts of vulcanizing agent, 1.5 parts of catalyst, 6 parts of accelerator, 2 parts of antioxidant, 5 parts of softener and 8 parts of flame retardant, wherein the flame retardant is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres.

[0048] The method for preparing the conveyor belt covering rubber provided by the present invention comprises the following steps:

[0049] Step 1, plasticizing: taking styrene-butadiene rubber, EPDM rubber, EPDM rubber and plasticizer stearate, putting them into an internal mixer, controlling the temperature at 150°C, and plasticizing to obtain a mixed rubber product;

[0050] Step 2, mixing: putting the accelerator zinc oxide, antioxidant, softener paraffin oil, reinforcing agent carbon black N234 and flame retardant montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material into the plasticizing rubber system, controlling the temperature and pressure of the reaction system, starting to discharge the glue at 135°C, repeatedly returning the glue after discharge, so that the components are evenly mixed, and then standing to cool, so that the mixed rubber sheet is cooled and shaped;

[0051] Step 3, vulcanization: put the film product in step 2 into the internal mixer, add the vulcanizing agent 1,1-bis(tert-butyl)-3,3,5-trimethylcyclohexane and the catalyst trimethylenediamine into the system, control the reaction time and system pressure, start the glue discharge when the temperature is maintained at 95°C, repeat the glue return operation to mix all the components evenly. Control the film thickness to 6mm and the film width to 600mm, and store it after cooling to 40°C.

[0052] The flame retardant used in the embodiment of the present invention is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres, and the preparation method comprises the following steps:

[0053] 1) Weigh 2.1g of montmorillonite and 0.9g of dihydroxydodecyltrimethylammonium chloride, add them into a 500ml three-necked flask, add 120ml of ethanol / water (mass ratio is 1 / 1) mixed dispersant, heat to 75℃, stir at 240r / min for 2.5h to obtain a swollen montmorillonite structure, then slowly drop 10ml of 1% sodium alginate solution into the solution, adjust the solution pH, control the speed at 260r / min, fully destroy the hydrogen bond structure between montmorillonite layers, then separate the solid and liquid, wash, dry in vacuum at 90℃, and grind to obtain exfoliated montmorillonite powder.

[0054] 2) 1.2 g of sodium dodecylbenzene sulfonate anionic surfactant, 0.6 g of calcium hydroxyphosphate, and 2.4 g of styrene were added to the reactor, nitrogen was introduced into the system to exhaust the air, and the system was stirred at 45°C at a high speed of 240 r / min. A mixed acid of sulfuric acid and nitric acid in a ratio of 3:2 was added. After reacting for 2 h, 0.02 g of initiator azobisisobutyl cyanide was added to the system, the magnetic stirring speed was controlled at 80 r / min, and the polymerization was initiated at 85°C for 2 h to obtain a nitropolystyrene microsphere solution grafted with anionic surfactant, which was recorded as solution A.

[0055] 3) Prepare MgCl2 for dissolution, adjust the pH of the solution with anhydrous ethanol and 0.5% hydrochloric acid solution, and prepare a mixed solution with a mass fraction of 4%. The resulting solution is recorded as solution B.

[0056] 4) Take 5 ml of solution A in a flask, add 30 ml of chloroform to disperse it, add the treated solution B to the solution A dispersed with chloroform, stir thoroughly to obtain a suspension of nitropolystyrene microspheres coated with hydrated magnesium chloride.

[0057] 5) Then the powder obtained in 1) is put into the suspension system, chloroform is added to fully disperse it, the temperature is controlled at 50°C, and ultrasonic treatment is performed for 20 minutes to allow the suspension microspheres and montmorillonite to form a uniform dispersion structure. Then 1% sodium sulfite solution is slowly added to the system, the temperature is controlled to be maintained at 60°C, and stirring is performed at a low speed of 70r / min. After reacting for 2 hours, it is allowed to stand to allow the microparticles and montmorillonite dispersion structure to solidify due to hybridization. The solvent is removed, the mixture is dried, and the powder with a dispersion structure of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is obtained by grinding.

[0058] Example 3

[0059] The conveyor belt covering rubber provided by the present invention comprises the following raw materials in parts by weight: 18 parts of styrene-butadiene rubber, 65 parts of ethylene-propylene-diene rubber, 27 parts of ethylene-propylene-diene rubber, 43 parts of reinforcing agent, 12 parts of plasticizer, 8 parts of vulcanizing agent, 1.5 parts of catalyst, 8 parts of accelerator, 1.5 parts of antioxidant, 7 parts of softener and 9 parts of flame retardant, wherein the flame retardant is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres.

[0060] The method for preparing the conveyor belt covering rubber provided by the present invention comprises the following steps:

[0061] Step 1, plasticizing: put styrene-butadiene rubber, EPDM rubber, EPDM rubber and plasticizer into an internal mixer, control the temperature at 155°C, and plasticize to obtain a mixed rubber product;

[0062] Step 2, mixing: putting the accelerator, antioxidant, softener, reinforcing agent and flame retardant montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material into the plasticizing rubber system, controlling the temperature and pressure of the reaction system, starting to discharge the glue at 130°C, repeatedly returning the glue after discharge, so that the components are evenly mixed, and then standing to cool, so that the mixed rubber sheet is cooled and shaped;

[0063] Step 3, vulcanization: put the film product in step 2 into an internal mixer, add vulcanizing agent and catalyst to the system, control the reaction time and system pressure, start to discharge the glue when the temperature is maintained at 98°C, repeat the glue return operation to mix the components evenly, control the film thickness to 7mm, the film width to 600mm, and store it after cooling to 40°C.

[0064] The flame retardant used in the embodiment of the present invention is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres, and the preparation method comprises the following steps:

[0065] 1) Weigh 2.1g of montmorillonite and 0.8g of dihydroxydodecyltrimethylammonium chloride, add them into a 500ml three-necked flask, add 120ml of ethanol / water (mass ratio is 1 / 1) mixed dispersant, heat to 77℃, stir at 250r / min for 2h to obtain a swollen montmorillonite structure, then slowly drop 10ml of 1.5% sodium alginate solution into the solution, adjust the solution pH, control the speed at 250r / min, fully destroy the hydrogen bond structure between the montmorillonite layers, then separate the solid and liquid, wash, dry in vacuum at 90℃, and grind to obtain exfoliated montmorillonite powder.

[0066] 2) 1.2 g of sodium dodecylbenzene sulfonate anionic surfactant, 0.6 g of calcium hydroxyphosphate, and 2.3 g of styrene were added to the reactor, nitrogen was introduced into the system to exhaust the air, and the system was stirred at 48°C at a high speed of 250 r / min. A mixed acid of sulfuric acid and nitric acid in a ratio of 3:2 was added. After reacting for 2 h, 0.02 g of initiator azobisisobutyl cyanide was added to the system, the magnetic stirring speed was controlled at 75 r / min, and the polymerization was initiated at 88°C for 2.5 h to obtain a nitropolystyrene microsphere solution grafted with anionic surfactant, which was recorded as solution A.

[0067] 3) Prepare MgCl2 for dissolution, adjust the pH of the solution with anhydrous ethanol and 0.5% hydrochloric acid solution, and prepare a mixed solution with a mass fraction of 5%. The resulting solution is recorded as solution B.

[0068] 4) Take 5 ml of solution A in a flask, add 30 ml of chloroform to disperse it, add the treated solution B to the solution A dispersed with chloroform, stir thoroughly to obtain a suspension of nitropolystyrene microspheres coated with hydrated magnesium chloride.

[0069] 5) Then the powder obtained in 1) is added to the suspension system, chloroform is added to fully disperse it, the temperature is controlled at 60°C, and ultrasonic treatment is performed for 25 minutes to allow the suspension microspheres and montmorillonite to form a uniform dispersion structure. Then 1% sodium sulfite solution is slowly added to the system, the temperature is controlled to be maintained at 55°C, and stirring is performed at a low speed of 75r / min. After reacting for 1.5 hours, it is allowed to stand to allow the microparticles and montmorillonite dispersion structure to solidify due to hybridization. The solvent is removed, the mixture is dried, and the powder of the dispersion structure of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is obtained by grinding.

[0070] Example 4

[0071] Compared with Example 3, the only difference is that the conveyor belt covering rubber raw materials used are different in the number of parts, namely, the raw materials include the following parts by weight: 16 parts of styrene-butadiene rubber, 66 parts of EPDM rubber, 29 parts of EPDM rubber, 41 parts of reinforcing agent, 12 parts of plasticizer, 8 parts of vulcanizing agent, 2 parts of catalyst, 6 parts of accelerator, 3 parts of antioxidant, 7 parts of softener, 9 parts of flame retardant, and the other components and steps remain unchanged.

[0072] Example 5

[0073] Compared with Example 3, the only difference is that the raw materials and the quantity of the conveyor belt covering rubber are different, namely, 18 parts of styrene-butadiene rubber, 69 parts of EPDM rubber, 27 parts of EPDM rubber, 43 parts of reinforcing agent, 11 parts of plasticizer, 6 parts of softener and 10 parts of flame retardant, and the other steps remain unchanged.

[0074] Comparative Example 1

[0075] Compared with Example 3, the only difference is that no exfoliated montmorillonite powder is used, that is, step 1) preparation of exfoliated montmorillonite powder is not performed, and only nitropolystyrene microspheres coated with hydrated magnesium chloride are used, and other components and steps remain unchanged.

[0076] Comparative Example 2

[0077] Compared with Example 3, the only difference is that the nitropolystyrene microsphere suspension coated with hydrated magnesium chloride is not used, that is, steps 2), 3), and 4) of preparing the nitropolystyrene microsphere suspension coated with hydrated magnesium chloride are not performed, only exfoliated montmorillonite powder is used, and other components and steps remain unchanged.

[0078] Comparative Example 3

[0079] Compared with Example 3, the difference is that the preparation of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite flame retardant is not carried out, and the flame retardant obtained by mixing zinc borate, antimony trioxide and flame retardant IFR in a weight ratio of 1:1:1 commonly used in the prior art is directly used to replace the flame retardant in Example 3, and the other components and steps remain unchanged.

[0080] Comparative Example 4

[0081] Compared with Comparative Example 3, the difference lies in the usage fraction of the flame retardant, that is, the usage fraction of the flame retardant obtained by mixing zinc borate, antimony trioxide and flame retardant IFR in a weight ratio of 1:1:1 commonly used in the prior art is 30 parts, and the other components and steps remain unchanged.

[0082] Performance tests were performed on finished conveyor belts prepared with the conveyor belt covering rubbers of Examples 1 to 5 and Comparative Examples 1 to 4. The test methods are shown in Table 1, and the test results are shown in Table 2.

[0083] Table 1 Performance test method table of Examples 1 to 5 and Comparative Examples 1 to 4

[0084]

[0085] Table 2 Performance test results of Examples 1 to 5 and Comparative Examples 1 to 4

[0086]

[0087] According to the data in Table 2 combined with Table 1, it can be seen that the conveyor belts prepared with the covering rubber obtained in Examples 1 to 5 of the present invention meet the requirements of the national standards for related properties such as tensile strength, elongation at break and burner combustion performance.

[0088] From the analysis of Table 2, it can be seen that the tensile strengths in Examples 1 to 5 are all higher than 15 MPa, the tensile strengths in Comparative Examples 1 to 3 are around 15 MPa, and the tensile strength in Comparative Example 4 is lower than 15 MPa. It can be seen that the use of a large amount of flame retardant will reduce the tensile strength of the conveyor belt. Compared with Example 3, Comparative Examples 1 and 2 respectively use nitrostyrene microspheres coated with hydrated magnesium chloride and exfoliated montmorillonite powder, and the flame retardant effect achieved is significantly reduced, and the tensile strength and other properties are deteriorated.

[0089] From the analysis of Table 2, it can be seen that Examples 1 to 5 and Comparative Example 4 meet the requirements of the national standard for burner combustion performance, while Comparative Examples 1 to 3 do not meet the requirements of the national standard for burner combustion performance. It can be seen that although the tensile strength and other indicators of Comparative Examples 1 to 3 meet the standards, the flame retardant performance is poor due to the small amount of flame retardant used, while the flame retardant performance of Comparative Example 4 meets the standards due to the large amount of flame retardant used, but the tensile strength and other indicators are poor.

[0090] In summary, the flame retardant used in this application is a montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material, which, combined with the other raw material components, can reduce the amount of flame retardant used while ensuring strong flame retardant properties and tensile strength.

[0091] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A whole core flame retardant conveyor belt covering rubber for coal mines, characterized in that: The invention comprises the following raw materials: styrene-butadiene rubber, ethylene-propylene-diene rubber, ethylene-propylene-diene rubber, a reinforcing agent, a plasticizer, a softener and a flame retardant, wherein the flame retardant is a composite material of montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microspheres; The montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material is prepared by the following steps: S1, using montmorillonite and bis(hydroxydodecyltrimethylammonium chloride) to swell to obtain a swollen montmorillonite structure, then adding sodium alginate solution dropwise, stirring, solid-liquid separation, and grinding to obtain montmorillonite powder; S2, using sodium dodecylbenzene sulfonate anionic surfactant, hydroxy calcium phosphate and styrene mixed with mixed acid and reacted, then adding initiator azobisisobutyl cyanide to initiate polymerization reaction to obtain solution A; dissolving MgCl2 to prepare a mixed solution, and the obtained solution is recorded as solution B; taking solution A, adding chloroform and solution B to obtain a suspension of nitro polystyrene microspheres coated with hydrated magnesium chloride; S3, adding the montmorillonite powder obtained in step S1, dropping the sodium sulfite solution, stirring, removing the solvent, drying, and grinding to obtain a montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material.

2. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 1 is characterized in that: When swelling is performed in S1, ethanol and water need to be added for heating and stirring. The mass ratio of ethanol to water is 1:1, the heating temperature is 75-80°C, the stirring time is 1.5-2.5h, the stirring rate is 240-260r / min, and the mass fraction of the sodium alginate solution is 1-2%.

3. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 1 is characterized in that: The reaction conditions after mixing in S2 include a temperature of 45-50° C., a stirring rate of 240-260 r / min, and a stirring time of 1.5-2.5 h; the conditions during the polymerization reaction include a temperature of 85-90° C., a stirring rate of 70-80 r / min, and a stirring time of 2-2.5 h.

4. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 1 is characterized in that: The mass fraction of the solute in the mixed solution in S2 is 4-6%, the mixed acid is sulfuric acid and nitric acid, and the mass ratio of sulfuric acid to nitric acid is 3:

2.

5. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 1 is characterized in that: After adding montmorillonite powder to the S3, ultrasonic dispersion is performed, the ultrasonic dispersion time is 20-30 minutes, and the ultrasonic dispersion temperature is 50-65° C.; when adding sodium sulfite solution, the low-speed stirring time is 1-2 hours, and the stirring rate is 70-80 r / min.

6. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 1 is characterized in that: It also includes vulcanizing agent, catalyst, accelerator and antioxidant. The weight proportions of each raw material are 15-20 parts of styrene-butadiene rubber, 60-70 parts of EPDM rubber, 25-30 parts of EPDM rubber, 40-45 parts of reinforcing agent, 10-15 parts of plasticizer, 5-10 parts of vulcanizing agent, 1.5-2 parts of catalyst, 5-7 parts of accelerator, 2-3 parts of antioxidant, 5-10 parts of softener and 8-10 parts of flame retardant.

7. The whole core flame retardant conveyor belt covering rubber for coal mine according to claim 6 is characterized in that: The reinforcing agent is carbon black N234; the plasticizer is stearate; the vulcanizing agent is 1,1-bis(tert-butyl)-3,3,5-trimethylcyclohexane; the catalyst is trimethylenediamine; the accelerator is zinc oxide; and the softener is paraffin oil.

8. A method for preparing the covering rubber of the whole core flame retardant conveyor belt for coal mines according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1, plasticizing: weighing styrene-butadiene rubber, EPDM rubber, EPDM rubber and plasticizer according to weight proportions, putting them into an internal mixer, and plasticizing to obtain a mixed rubber product; Step 2, mixing: putting the accelerator, antioxidant, softener, reinforcing agent and montmorillonite-sulfonated nitropolystyrene-hydrated magnesium chloride microsphere composite material into the plasticizing rubber system, repeatedly returning the glue after the glue is discharged to make the components evenly mixed, and then standing and cooling to make the mixed rubber sheet cool and set; Step 3: Vulcanization: Put the film product in step 2 into an internal mixer, add a vulcanizing agent and a catalyst into the system, control the reaction time and temperature, repeatedly return the glue after debinding, mix all the components evenly, and obtain a covering rubber film.

9. The method for preparing the covering rubber of the whole core flame retardant conveyor belt for coal mine according to claim 8, characterized in that: The temperature during plastication is controlled at 150-160°C, the mixing and debonding temperature range is 125-135°C; the vulcanization debonding temperature is 95-100°C; and the thickness of the covering rubber sheet is 6-7mm.