Gypsum powder for jewelry processing and preparation method thereof

By combining modified kaolin with nano-silica, combined with silane coupling agent modification and adding stabilizers, the problems of poor high temperature resistance and low compressive strength of traditional gypsum powder in jewelry processing have been solved, and the performance of gypsum powder has been significantly improved. mechanical properties and processing quality.

CN118515461BActive Publication Date: 2024-10-15GUANGZHOU HONGJING JEWELRY FOUNDRY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982192.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Traditional gypsum powder has problems in jewelry processing such as poor high temperature resistance, low compressive strength, and prone to cracks and pores, which affects processing quality and efficiency.

Method used

Modified kaolin is combined with nano-silica, modified through hydrothermal reaction and silane coupling agent, and stabilizer, water reducing agent and retarder are added to improve the high temperature resistance and compressive strength of gypsum powder and reduce the risk of cracking .

Benefits of technology

Significantly improves the initial and final setting rates of gypsum powder, forms a dense microstructure, enhances mechanical properties, ensures that the mold does not deform during high-temperature baking, reduces cracks and pores, and improves the integrity and service life of the mold.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a gypsum powder for jewelry processing and a preparation method thereof, and relates to the technical field of gypsum materials. The gypsum powder for jewelry processing of the present invention comprises the following materials in parts by weight: 100 parts of α-gypsum powder, 8-12 parts of modified kaolin, 2-3 parts of stabilizer, 2.5-3.5 parts of water reducer, 1.5-2.5 parts of enhancer, and 0.5-1 part of retarder. The gypsum powder for jewelry processing of the present invention improves the high temperature resistance and compressive strength of the gypsum powder by adjusting the ratio of each component, and also reduces the cracking of the gypsum powder; the preparation method provided has the advantages of low raw material cost, simple preparation process, high production efficiency, etc., and can meet the requirements of the modern jewelry processing industry for the performance of gypsum powder; at the same time, the preparation method also has the characteristics of environmental protection and energy saving, which conforms to the development trend of green manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gypsum materials, and in particular to gypsum powder used for jewelry processing and a preparation method thereof. Background Art

[0002] In the jewelry processing industry, gypsum powder is an important auxiliary material, and its quality and performance directly affect the quality and efficiency of jewelry processing. Traditional gypsum powder has many problems in the jewelry processing process, such as poor high temperature resistance, low compressive strength, easy to produce cracks and pores, etc. These problems not only reduce the quality of jewelry processing, but also increase processing costs and time.

[0003] First, traditional gypsum powder is prone to deformation and cracking in high temperature environments, which makes jewelry molds easily damaged during the firing process and reduces the service life of the molds. At the same time, such deformation and cracking will also affect the precision and surface quality of jewelry. Secondly, the compressive strength of traditional gypsum powder is low, which makes the gypsum molds easily broken by external forces during the jewelry casting process, resulting in the scrapping of castings and waste of materials. In addition, traditional gypsum powder is prone to pores and impurities during the preparation process, which will affect the density and precision of the gypsum molds, and thus affect the quality and precision of jewelry castings.

[0004] Based on this, the present invention provides a gypsum powder for jewelry processing and a preparation method thereof. Summary of the invention

[0005] The purpose of the present invention is to provide a gypsum powder for jewelry processing and a preparation method thereof, which improves the high temperature resistance and compressive strength of the gypsum powder and reduces the cracking of the gypsum powder.

[0006] On the one hand, the present invention provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 8-12 parts of modified kaolin, 2-3 parts of stabilizer, 2.5-3.5 parts of water reducer, 1.5-2.5 parts of enhancer, and 0.5-1 part of retarder.

[0007] Furthermore, the preparation method of the modified kaolin includes: adding kaolin and nano-silicon dioxide into water and mixing them with ultrasound, subjecting the ultrasonically obtained material to a hydrothermal reaction in a hydrothermal reactor, drying it for the first time after vacuum filtration, and then grinding it to obtain a composite material; adding a silane coupling agent to a methanol aqueous solution with a mass fraction of 95%, adding the composite material under stirring in a water bath, continuing to stir, drying it for the second time, and grinding it to obtain the modified kaolin.

[0008] Furthermore, the usage ratio of kaolin, nano-silicon dioxide and water is (2-4) g: (5-9) g: (50-60) mL.

[0009] Furthermore, the kaolin is calcined kaolin, the calcination temperature is 500-560° C., and the calcination time is 4-5 hours.

[0010] Furthermore, the temperature of the ultrasonic compounding is 60-70° C., and the time of the ultrasonic compounding is 2-3 hours.

[0011] Furthermore, the temperature of the hydrothermal reaction is 100-110° C., and the reaction time is 4-5 h.

[0012] Furthermore, the first drying temperature is 95-105° C., and the drying time is 2-3 hours; the second drying temperature is 50-60° C., and the drying time is 4-6 hours.

[0013] Furthermore, the silane coupling agent includes at least one of KH560 and KH570.

[0014] Furthermore, the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:(1-1.2):(50-60).

[0015] Furthermore, the temperature of the water bath is 65-75° C., and the stirring time of the water bath is 16-20 min.

[0016] Furthermore, the stabilizer is hydroxypropyl methylcellulose; the water reducer includes polycarboxylate water reducer PCE and polycarboxylate water reducer MNP-CP in a weight ratio of 1: (0.5-1).

[0017] Furthermore, the reinforcing agent is polypropylene fiber with a length of 6-10 mm; and the retarder is sodium citrate.

[0018] On the other hand, the present invention also provides a method for preparing gypsum powder for jewelry processing, the steps comprising:

[0019] (1) Preparation of modified kaolin;

[0020] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain the main material;

[0021] (3) Add stabilizer, water reducer, reinforcing agent and retarder to the main material and mix them to obtain the gypsum powder.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention adds modified kaolin to the main material to promote the hydration reaction of gypsum. When the modified kaolin is mixed with gypsum powder, the initial and final setting rates of gypsum can be significantly improved. Modified kaolin and gypsum can form a denser microstructure, improve the overall mechanical properties, and maintain stable performance under high temperature environment, ensuring that the mold does not deform or break during high-temperature roasting. In addition, the gypsum powder after adding modified kaolin has a higher compressive strength, which can meet the requirements of high-precision jewelry processing for mold strength. It also effectively reduces the generation of cracks and pores when using it to prepare gypsum molds, thereby improving the integrity and service life of the mold.

[0024] (2) In the present invention, kaolin is first calcined, the main purpose of which is to remove the moisture inside it and the hydroxyl groups in the structure, so as to change the crystal structure. The calcined kaolin usually has the characteristics of higher whiteness, reduced density, increased specific surface area, increased oil absorption, and improved thermal stability; the calcined kaolin has enhanced thermal stability, and when compounded with gypsum powder, it can improve the high temperature resistance of the overall material; when the structure of kaolin changes, it can also form a more stable support structure, which helps to improve the compressive strength of the composite material, and the microstructural changes of kaolin after calcination can also reduce the stress concentration points inside the material, thereby reducing the risk of cracking.

[0025] (3) In the present invention, nano-silicon dioxide is added to kaolin. Since nano-silicon dioxide has an extremely small particle size and a high specific surface area, compounding it with kaolin can significantly improve the microstructure and performance of the material. Nano-silicon dioxide can fill the gaps between kaolin particles, forming a denser structure and enhancing the interaction between particles. The introduction of silane coupling agent modification further enhances the interaction between inorganic fillers and organic matrices. This strong interface bonding can reduce the thermal expansion rate of the gypsum mixture, improve the dimensional stability of the material, and help improve the high temperature resistance of the overall material, that is, improve the temperature resistance of the gypsum powder.

[0026] (4) The present invention uses polycarboxylate water reducer PCE and polycarboxylate water reducer MNP-CP for compounding to further enhance the water reduction effect, so that the amount of water required for gypsum powder at the same fluidity is reduced, thereby reducing the water-to-paste ratio. In the prior art, polycarboxylate water reducer, naphthalene water reducer or polyamide water reducer are usually used for compounding, but in the selection of gypsum powder raw materials, the modified kaolin prepared by the present invention is added, and PCE and MNP-CP are selected in the polycarboxylate water reducer to produce a synergistic effect. Through surface adsorption and electrostatic repulsion, gypsum particles can be effectively dispersed, and the fluidity and plasticity of the gypsum slurry can be improved; it can also improve the microstructure of the gypsum hardened body, reduce the porosity, and refine the pore size, thereby improving the crack resistance of gypsum products.

[0027] (5) In the present invention, hydroxypropyl methylcellulose is selected as a stabilizer, polypropylene fiber with a length of 6-10 mm is selected as a reinforcing agent, sodium citrate is selected as a retarder, and the proportions of various raw materials are adjusted, thereby improving the high temperature resistance and compressive strength of the gypsum powder and reducing the cracking of the gypsum powder. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. It should be noted that the raw materials can be obtained commercially.

[0029] In the embodiment of the present invention, the water reducer is polycarboxylate water reducer PCE and polycarboxylate water reducer MNP-CP. The reinforcing agent is polypropylene fiber with a length of 6-10 mm; and the retarder is sodium citrate.

[0030] The polycarboxylate water reducer PCE in the embodiment of the present invention is a light reddish brown liquid with a solid content of 40%, purchased from Shanghai Sanrui Polymer Materials Co., Ltd.; the polycarboxylate water reducer MNP-CP is a powder purchased from Beijing Muhu Building Materials Sales Company; and the polypropylene fiber is purchased from Chongqing Xinsiwei Company.

[0031] Example 1

[0032] This embodiment provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0033] The preparation method of gypsum powder for jewelry processing in this embodiment comprises the following steps:

[0034] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0035] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0036] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0037] Example 2

[0038] This embodiment provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 8 parts of modified kaolin, 2 parts of stabilizer, 2.5 parts of water reducer, 1.5 parts of reinforcing agent, and 0.5 parts of retarder;

[0039] The preparation method of gypsum powder for jewelry processing in this embodiment comprises the following steps:

[0040] (1) Preparation of modified kaolin: First, calcining kaolin at 500°C for 4 h, adding the calcined kaolin and nano-silicon dioxide into water, mixing, and ultrasonicating at 60°C for 2 h; wherein the amount ratio of the calcined kaolin, nano-silicon dioxide, and water is (2) g: (5) g: (50) mL; the ultrasonically obtained material is subjected to hydrothermal reaction at 100°C for 4 h in a hydrothermal reactor, filtered under reduced pressure, and then dried for the first time at 95°C. The drying time is 2 hours, and then the composite material is obtained by grinding; the silane coupling agent KH570 is added to a methanol aqueous solution with a mass fraction of 95%, and the composite material is added after stirring in a water bath at a temperature of 65°C for 16 minutes, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1:50, and the stirring is continued for 10 minutes, and the solid sediment is centrifuged after cooling, and washed with anhydrous methanol, and dried for a second time at a temperature of 50°C for 4 hours, and then ground to obtain the composite material;

[0041] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0042] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:(0.5).

[0043] Example 3

[0044] This embodiment provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 12 parts of modified kaolin, 3 parts of stabilizer, 3.5 parts of water reducer, 2.5 parts of reinforcing agent, and 1 part of retarder;

[0045] The preparation method of gypsum powder for jewelry processing in this embodiment comprises the following steps:

[0046] (1) Preparation of modified kaolin: First, calcining kaolin at 560°C for 5 h, adding the calcined kaolin and nano-silicon dioxide into water, mixing, and ultrasonicating at 70°C for 3 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide, and water is (4) g: (9) g: (60) mL; the ultrasonically obtained material is subjected to hydrothermal reaction at 110°C for 5 h in a hydrothermal reactor, filtered under reduced pressure, and then dried for the first time at 105°C. The drying time is 3 hours, and then grinding is performed to obtain a composite material; the silane coupling agent KH560 is added to a methanol aqueous solution with a mass fraction of 95%, and the composite material is added after stirring in a water bath at a temperature of 75°C for 20 minutes, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.2:60, and the stirring is continued for 12 minutes. After cooling, centrifugation is performed, and the solid sediment is washed with anhydrous methanol, and a second drying is performed at a temperature of 60°C for 6 hours, and then grinding is performed to obtain;

[0047] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0048] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:1.

[0049] Example 4

[0050] This embodiment provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 12 parts of modified kaolin, 2 parts of stabilizer, 3.5 parts of water reducer, 1.5 parts of reinforcing agent, and 1 part of retarder;

[0051] The preparation method of gypsum powder for jewelry processing in this embodiment comprises the following steps:

[0052] (1) Preparation of modified kaolin: First, calcining kaolin at 500°C for 5 h, adding the calcined kaolin and nano-silicon dioxide into water, mixing, and ultrasonicating at 60°C for 3 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water is (2) g: (9) g: (50) mL; the ultrasonically obtained material is subjected to hydrothermal reaction at 110°C for 4 h in a hydrothermal reactor, filtered under reduced pressure, and then dried for the first time at 105°C. The drying time is 2 hours, and then the composite material is obtained by grinding; the silane coupling agent KH570 is added to a methanol aqueous solution with a mass fraction of 95%, and the composite material is added after stirring in a water bath at a temperature of 75°C for 16 minutes, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1:60, and the stirring is continued for 12 minutes, and the solid sediment is centrifuged after cooling, and the solid sediment is washed with anhydrous methanol, and the solid sediment is dried for a second time at a temperature of 50°C for 6 hours, and then ground to obtain the composite material;

[0053] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0054] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0055] Comparative Example 1

[0056] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0057] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0058] Preparation of modified kaolin: first, calcining kaolin at a temperature of 530°C for 4.5h, adding the calcined kaolin and nano-silicon dioxide into water and mixing them, and then ultrasonicating them at 65°C for 2.5h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water is 3g:7g:55mL; the material obtained by ultrasonication is subjected to hydrothermal reaction at 105°C in a hydrothermal reactor for 4.5h, and after vacuum filtration, it is dried for the first time at 100°C for 2.5h, and then ground to obtain a composite material; mixing the silane coupling agent KH560 with a weight ratio of 10:1.1 with the composite material, adding it to a ball mill, and grinding it for 60min to obtain;

[0059] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0060] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0061] Comparative Example 2

[0062] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0063] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0064] (1) Preparation of modified kaolin: First, calcining kaolin at 530°C for 4.5h, adding the calcined kaolin and nano-silica into water, mixing, and ultrasonicating at 65°C for 2.5h; wherein the amount ratio of calcined kaolin, nano-silica and water is 3g:7g:55mL; the ultrasonically obtained material is subjected to hydrothermal reaction at 105°C in a hydrothermal reactor for 4.5h, filtered under reduced pressure, and dried for the first time at 100°C for 2.5h, and then ground to obtain a composite material; 1g of the composite material is added to 10mL of a 10% sulfuric acid solution, stirred for 15min, and then allowed to stand for activation for 24h, filtered under reduced pressure, and dried for the second time at 55°C for 4.5h, and then ground to obtain;

[0065] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0066] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0067] Comparative Example 3

[0068] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0069] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0070] (1) Preparation of modified kaolin: First, calcining kaolin at 530°C for 4.5h, adding the calcined kaolin and nano-silica into water, mixing, and ultrasonicating at 65°C for 2.5h; wherein the amount ratio of calcined kaolin, nano-silica and water is 3g:7g:55mL; the material obtained by ultrasonication is subjected to hydrothermal reaction at 105°C for 4.5h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C for 2.5h, and then ground to obtain a composite material; 1g of the composite material is added to 10mL of a 10% sodium hydroxide solution, stirred for 15min, and then allowed to stand for activation for 24h, filtered under reduced pressure, and dried for the second time at 55°C for 4.5h, and then ground to obtain;

[0071] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0072] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0073] Comparative Example 4

[0074] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0075] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0076] (1) Preparation of modified kaolin: First, calcining kaolin at 530°C for 4.5 hours, adding the calcined kaolin and nano-silicon dioxide into water, mixing, and ultrasonicating at 65°C for 2.5 hours; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water is 3g:7g:55mL; the material obtained by ultrasonication is subjected to hydrothermal reaction at 105°C in a hydrothermal reactor for 4.5 hours, and after vacuum filtration, it is dried for the first time at 100°C for 2.5 hours, and then ground to obtain the product;

[0077] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0078] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0079] Comparative Example 5

[0080] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0081] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0082] (1) Preparation of modified kaolin: kaolin and nano-silica were added to water and mixed, and then ultrasonicated at 65°C for 2.5 hours; wherein the amount ratio of kaolin, nano-silica and water was 3g:7g:55mL; the material obtained by ultrasonication was subjected to hydrothermal reaction in a hydrothermal reactor at 105°C for 4.5 hours, and after vacuum filtration, it was dried for the first time at 100°C for 2.5 hours, and then ground to obtain a composite material; silane coupling agent KH560 was added to a methanol aqueous solution with a mass fraction of 95%, and stirred in a water bath at 70°C for 18 minutes, and then the composite material was added, wherein the weight ratio of the composite material, silane coupling agent and methanol aqueous solution was 10:1.1:55, and the stirring was continued for 11 minutes. After cooling, the solid sediment was centrifuged, washed with anhydrous methanol, and dried for the second time at 55°C for 4.5 hours, and then ground to obtain;

[0083] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0084] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0085] Comparative Example 6

[0086] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0087] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0088] (1) Preparation of modified kaolin: first, calcining kaolin at 530°C for 4.5h, adding silane coupling agent KH560 to a 95% by mass methanol aqueous solution, stirring in a water bath at 70°C for 18min, and then adding the calcined kaolin, wherein the weight ratio of the calcined kaolin, silane coupling agent and methanol aqueous solution is 10:1.1:55, stirring is continued for 11min, cooling and centrifuging are performed, and the solid sediment is washed with anhydrous methanol, dried for a second time at 55°C for 4.5h, and then ground to obtain the modified kaolin;

[0089] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0090] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0091] Comparative Example 7

[0092] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0093] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0094] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0095] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, polycarboxylate water reducer PCE, reinforcing agent polypropylene fiber and retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0096] Comparative Example 8

[0097] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0098] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0099] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0100] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, polycarboxylate water reducer MNP-CP, reinforcing agent polypropylene fiber and retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0101] Comparative Example 9

[0102] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0103] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0104] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0105] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0106] The water reducer is a polycarboxylate water reducer PCE and a FDN naphthalene water reducer in a weight ratio of 1:0.7.

[0107] Comparative Example 10

[0108] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0109] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0110] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0111] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer methyl cellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0112] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0113] Comparative Example 11

[0114] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0115] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0116] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0117] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent carbon fiber and a retarder sodium citrate to the main material and mixing them to obtain the gypsum powder.

[0118] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0119] Comparative Example 12

[0120] This comparative example provides a gypsum powder for jewelry processing, comprising the following materials in parts by weight: 100 parts of α-gypsum powder, 10 parts of modified kaolin, 2.5 parts of stabilizer, 3 parts of water reducer, 2 parts of reinforcing agent, and 0.7 parts of retarder;

[0121] The preparation method of gypsum powder for jewelry processing in this comparative example comprises the following steps:

[0122] (1) Preparation of modified kaolin: First, calcined kaolin at 530°C for 4.5 h, added the calcined kaolin and nano-silicon dioxide into water, mixed them, and then ultrasonicated them at 65°C for 2.5 h; wherein the amount ratio of calcined kaolin, nano-silicon dioxide and water was 3 g:7 g:55 mL; the ultrasonicated material was subjected to hydrothermal reaction at 105°C for 4.5 h in a hydrothermal reactor, filtered under reduced pressure, and dried for the first time at 100°C. The time interval is 2.5 hours, and then grinding to obtain a composite material; adding silane coupling agent KH560 to a methanol aqueous solution with a mass fraction of 95%, stirring in a water bath at a temperature of 70°C for 18 minutes, and then adding the composite material, wherein the weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:1.1:55, continuing to stir for 11 minutes, cooling and centrifuging, washing the solid sediment with anhydrous methanol, drying for a second time at a temperature of 55°C for 4.5 hours, and then grinding to obtain;

[0123] (2) Weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; adding stabilizer hydroxypropyl methylcellulose, a water reducer, a reinforcing agent polypropylene fiber and a retarder sodium gluconate to the main material and mixing them to obtain the gypsum powder.

[0124] The water reducer is a polycarboxylate water reducer PCE and a polycarboxylate water reducer MNP-CP in a weight ratio of 1:0.7.

[0125] Test Example 1: The performance of the gypsum powder for jewelry processing prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-12 was investigated.

[0126] Test method: The test process of setting time is carried out in accordance with GB / T17669.4-1999 "Determination of physical properties of building gypsum paste"; 2h flexural strength and dry compressive strength are carried out in accordance with GB / T28627-2012 "Plastering gypsum" test method.

[0127] The performance test results are shown in Table 1 below:

[0128] Table 1 Performance test

[0129]

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A gypsum powder for jewelry processing, characterized in that: The composition is composed of the following materials in parts by weight: 100 parts of α-gypsum powder, 8-12 parts of modified kaolin, 2-3 parts of stabilizer, 2.5-3.5 parts of water reducer, 1.5-2.5 parts of reinforcing agent, and 0.5-1 parts of retarder; The preparation method of the modified kaolin comprises: adding kaolin and nano-silicon dioxide into water, mixing them by ultrasound, carrying out hydrothermal reaction of the ultrasonically obtained material in a hydrothermal reaction kettle, drying for the first time after vacuum filtration, and then grinding to obtain a composite material; adding a silane coupling agent into a methanol aqueous solution with a mass fraction of 95%, adding the composite material under stirring in a water bath, continuing stirring, drying for the second time, and grinding to obtain the modified kaolin; the temperature of the hydrothermal reaction is 100-110° C., and the reaction time is 4-5 hours; The kaolin is calcined kaolin at a temperature of 500-560° C. for a calcination time of 4-5 h; The stabilizer is hydroxypropyl methylcellulose; the water reducer includes polycarboxylate water reducer PCE and polycarboxylate water reducer MNP-CP in a weight ratio of 1: (0.5-1); The reinforcing agent is polypropylene fiber with a length of 6-10 mm; the retarder is sodium citrate.

2. The gypsum powder for jewelry processing according to claim 1, characterized in that: The dosage ratio of the kaolin, nano-silicon dioxide and water is (2-4) g: (5-9) g: (50-60) mL.

3. The gypsum powder for jewelry processing according to claim 1, characterized in that: The weight ratio of the composite material, the silane coupling agent and the methanol aqueous solution is 10:(1-1.2):(50-60).

4. The gypsum powder for jewelry processing according to claim 1, characterized in that: The temperature of the water bath is 65-75° C., and the stirring time of the water bath is 16-20 min.

5. A method for preparing gypsum powder for jewelry processing according to any one of claims 1 to 4, characterized in that the steps include: (1) Preparation of modified kaolin; (2) weighing raw materials as required, mixing α-gypsum powder and modified kaolin to obtain a main material; (3) adding a stabilizer, a water reducer, a reinforcing agent and a retarder to the main material and mixing them to obtain the gypsum powder.