LED epitaxial wafer and preparation method thereof, LED

By adopting the design of multi-layer structure and composite quantum barrier layer in LED epitaxial wafers, the problem of low LED luminous efficiency at small current densities is solved, and efficient light emission and carrier recombination at small current densities are achieved.

CN118522833BActive Publication Date: 2024-10-29JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410985761.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-29
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing LEDs have low luminous efficiency at low current densities, and the epitaxial structure design and growth methods are difficult to take into account the device luminous efficiency at both low and high current densities.

Method used

An LED epitaxial wafer structure including a substrate, a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum well layer and a P-type semiconductor layer is used. The multi-quantum well layer consists of alternately stacked InGaN quantum well layers and composite quantum barrier layers. Composed, the composite quantum barrier layer is composed of N-type GaN, N-type AlGaN, N-type GaN and N-type InGaN layers are stacked in sequence. The growth temperature of the quantum well layer first decreases and then increases. The growth rate of the composite quantum barrier layer decreases, forming a gradient energy system to optimize hole injection. efficiency and carrier recombination.

Benefits of technology

It improves the luminous efficiency under small current density, optimizes the hole injection path, limits carrier overflow, improves crystal quality and turn-on voltage, and enhances the radiative recombination efficiency under small current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118522833B_ABST
    Figure CN118522833B_ABST
Patent Text Reader

Abstract

This invention discloses an LED epitaxial wafer and its fabrication method, as well as an LED, relating to the field of semiconductor technology. The LED epitaxial wafer comprises a multi-quantum-well layer including at least three sub-layers, each sub-layer including periodically alternating InGaN quantum well layers and a composite quantum barrier layer; the composite quantum barrier layer includes a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer, and an N-type InGaN layer stacked sequentially; the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer; along the epitaxial growth direction, the growth temperature of the quantum well layers in different sub-layers first decreases and then increases. Implementing this invention can improve the luminous efficiency of LEDs at low current densities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to an LED epitaxial wafer and a preparation method thereof, and an LED. Background Art

[0002] In recent years, Group III nitride semiconductors represented by GaN-based materials have been widely used in lighting devices, mobile phone backlights, instruments, traffic lights, outdoor displays and other fields due to their wide bandgap, direct band gap, high electron mobility and high thermal conductivity.

[0003] The goal of epitaxial structure design and material growth for conventional chips for general lighting and backlight display applications is usually to achieve high current density (20A / cm 2 ~100A / cm 2 ) and cannot take into account the light efficiency at low current density (less than 20A / cm 2 ) under low current density. The design of epitaxial layer structure and the regulation of growth method have a great effect and influence on the hole injection path and injection efficiency under low current density. Under low current density, the carrier concentration in the quantum well is relatively low, the tunneling rate of carriers is greater than the rate of carrier recombination, and carriers are easily captured by deep energy level defects in the quantum well region. Therefore, the non-radiative recombination related to defects under low current density is the main reason affecting the internal quantum efficiency, while the non-radiative recombination effect caused by defects under high current density accounts for a relatively small proportion. In addition, the carrier overflow phenomenon is significantly weakened or does not occur under low current density. The electron blocking layer set to prevent electron overflow not only fails to block electrons under low current density, but also affects the efficiency of hole injection into the quantum well region and reduces the probability of carrier radiative recombination in the quantum well. In summary, the epitaxial structure and growth method of LEDs under low current density working conditions are essentially different from those under high current density. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an LED epitaxial wafer capable of improving the luminous efficiency under low current density.

[0005] Another technical problem to be solved by the present invention is to provide a method for preparing an LED epitaxial wafer, and the prepared LED has high luminous efficiency.

[0006] In order to solve the above problems, the present invention discloses an LED epitaxial wafer, comprising a substrate and a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer sequentially deposited on the substrate, wherein the multi-quantum well layer comprises at least three sublayers, each of which comprises a quantum well layer and a composite quantum barrier layer that are periodically and alternately stacked;

[0007] The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer comprises a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence; the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer;

[0008] Along the epitaxial growth direction, the growth temperature of the quantum well layer in different sub-layers first decreases and then increases.

[0009] As an improvement of the above technical solution, the number of sublayers of the multi-quantum well layer is 3 to 20, and each sublayer includes a periodic structure in which 1 to 10 quantum well layers and composite quantum barrier layers are alternately grown.

[0010] As an improvement of the above technical solution, the thickness of the multi-quantum well layer is 100nm~300nm; in each period of each sub-layer, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:(3~5).

[0011] As an improvement of the above technical solution, the N-type doping concentration of the composite quantum barrier layer is 1×10 17 cm -3 ~1×10 18 cm -3 ;

[0012] In each composite quantum barrier layer, the N-type doping concentration of the first N-type GaN layer is the same as that of the N-type AlGaN layer, the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is the same, and the ratio of the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer to the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is (2~5):1.

[0013] As an improvement of the above technical solution, along the epitaxial growth direction, the thickness ratio of the quantum well layer and the composite quantum barrier layer in different sub-layers is reduced.

[0014] As an improvement of the above technical solution, the difference in growth temperature of the quantum well layer of two adjacent sub-layers is 0.5°C to 3°C.

[0015] As an improvement of the above technical solution, along the epitaxial growth direction, the growth rate of the composite quantum barrier layer in different sub-layers decreases.

[0016] Correspondingly, the present invention also discloses a method for preparing an LED epitaxial wafer, which is used to prepare the above-mentioned LED epitaxial wafer, comprising the following steps:

[0017] A substrate is provided, and a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer are sequentially grown on the substrate, wherein the multi-quantum well layer includes at least three sublayers, and each sublayer includes a quantum well layer and a composite quantum barrier layer that are periodically and alternately stacked;

[0018] The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer comprises a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence; the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer;

[0019] Along the epitaxial growth direction, the growth temperature of the quantum well layer in different sub-layers first decreases and then increases.

[0020] As an improvement of the above technical solution, the growth temperature of the quantum well layer is 790° C. to 810° C., and the growth pressure is 50 Torr to 300 Torr;

[0021] The growth temperature of the composite quantum barrier layer is 800° C. to 1000° C., and the growth pressure is 50 Torr to 300 Torr.

[0022] Correspondingly, the present invention also discloses an LED, which includes the above-mentioned LED epitaxial wafer.

[0023] The implementation of the present invention has the following beneficial effects:

[0024] 1. In the multi-quantum well layer of the present invention, along the epitaxial growth direction, the growth temperature of the quantum well layer in different sublayers first decreases and then increases. The sublayer with a lower growth temperature has a relatively low ground state energy level, and holes will preferentially fill into the quantum well layer with a low ground state energy level to undergo radiative recombination with electrons; the sublayer with a higher growth temperature has a relatively high ground state energy level, and it is difficult for the carriers that have been injected into the main light-emitting area to escape to the period with a higher ground state energy level, ultimately achieving the effect of optimizing the hole injection efficiency, while limiting the overflow of carriers to the side of the P-type semiconductor for non-radiative recombination.

[0025] 2. The composite quantum barrier layer of the present invention is formed by stacking N-type GaN layer, N-type AlGaN layer, N-type GaN and N-type InGaN layer in sequence to form a gradient energy system from low to high and then to low, so that the energy system of the bottom of the composite quantum barrier conduction band is higher than the energy system of the bottom of the quantum well conduction band, effectively localizing electrons in the quantum well, and increasing the probability of radiation recombination of electron holes in the quantum well. In addition, in the N-type AlGaN layer, the lattice constant of Al is small and the mobility is low, which can fully fill the deep energy level defects caused by lattice mismatch in the quantum well layer, reduce the defect density under small current injection, and improve the product crystal quality and turn-on voltage.

[0026] 3. In the multi-quantum well layer of the present invention, the growth rate of the composite quantum barrier layer in different sub-layers decreases along the epitaxial growth direction. The growth rate of the composite quantum barrier layer close to the N-type semiconductor layer is increased, and the growth mode tends to a 3D state, while the growth rate of the composite quantum barrier layer close to the P-type semiconductor layer is reduced, and the growth mode tends to a 2D state, which ultimately makes the morphology of the pits opened in the multi-quantum well layer closer to a U-shaped state, improves the hole injection path, and enhances the crystal quality in the effective radiation recombination area under low current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a structural schematic diagram of an LED epitaxial wafer provided by the present invention;

[0028] Figure 2 The present invention is a flow chart of the method for preparing an LED epitaxial wafer. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0030] See also Figure 1 The present invention provides an LED epitaxial wafer, comprising a substrate 1 and a buffer layer 2, an N-type semiconductor layer 3, a stress release layer 4, a multi-quantum well layer 5 and a P-type semiconductor layer 6 sequentially deposited on the substrate 1, wherein the multi-quantum well layer comprises at least three sublayers, and each sublayer comprises a quantum well layer and a composite quantum barrier layer that are periodically and alternately stacked.

[0031] In each period, the quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer includes a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence.

[0032] The composite quantum barrier layer is stacked in sequence by the first N-type GaN layer, the N-type AlGaN layer, the second N-type GaN and the N-type InGaN layer to form a gradient energy system from low to high and then to low, so that the energy system of the bottom of the composite quantum barrier conduction band is higher than the energy system of the bottom of the quantum well conduction band, effectively localizing the electrons in the quantum well and increasing the probability of radiation recombination of electron holes in the quantum well. In addition, the composite quantum barrier layer includes an N-type AlGaN layer, and the Al component accounts for 0.01~0.25. Due to the small lattice constant and low mobility of Al, it can fully fill the deep energy level defects caused by lattice mismatch in the quantum well layer. The reduction of defect density under small current injection greatly improves the product crystal quality and turn-on voltage.

[0033] Among them, the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer. By setting the N-type doping concentration in the composite quantum barrier layer, it is not easy for the electrons moving into the quantum well to reverse tunnel, while reducing the hole blocking barrier, improving the matching degree between electrons and holes, and finally improving the effective radiation recombination efficiency while reducing the operating voltage.

[0034] Along the epitaxial growth direction, the growth temperature of the quantum well layer in different sublayers decreases first and then increases. In the sublayer with a lower growth temperature, the ground state energy level is relatively low, and holes will preferentially fill the quantum well layer with a low ground state energy level to undergo radiative recombination with electrons; in the sublayer with a higher growth temperature, the ground state energy level is relatively high, and it is difficult for the carriers that have been injected into the main light-emitting area to escape to the period with a higher ground state energy level, ultimately achieving the effect of optimizing the hole injection efficiency, while limiting the overflow of carriers to the P-type semiconductor side for non-radiative recombination.

[0035] Preferably, the difference in growth temperature of the quantum well layer of two adjacent sublayers is 0.5°C to 3°C, exemplarily 0.8°C, 1°C, 1.5°C, 2°C or 2.5°C, but not limited thereto. The difference in growth temperature of the quantum well layer of two adjacent sublayers is controlled within a reasonable range, which will not adversely affect the crystal quality while improving the carrier recombination efficiency. Exemplarily, the growth temperature of the quantum well layer of the first sublayer is 801°C, the growth temperature of the quantum well layer of the second sublayer is 800°C, and the growth temperature of the quantum well layer of the third sublayer is 801°C, but not limited thereto.

[0036] In one embodiment, the growth rate of the composite quantum barrier layer in different sublayers decreases along the epitaxial growth direction. The growth rate of the composite quantum barrier layer near the N-type semiconductor layer is increased, and the growth mode tends to a 3D state; the growth rate of the composite quantum barrier layer near the P-type semiconductor layer is reduced, and the growth mode tends to a 2D state, and finally the morphology of the pits opened in the multi-quantum well layer is closer to a U-shaped state, the hole injection path is improved, and the crystal quality in the effective radiation recombination area under low current density is enhanced.

[0037] Specifically, the number of sublayers of the multi-quantum well layer is 3 to 20, and is exemplarily 4, 5, 8, 10 or 15, but is not limited thereto. Each sublayer includes a periodic structure in which 1 to 10 quantum well layers and composite quantum barrier layers are alternately grown. The thickness of the multi-quantum well layer is 100 nm to 300 nm, and is exemplarily 120 nm, 150 nm, 180 nm, 200 nm or 250 nm, but is not limited thereto.

[0038] In one embodiment, in each period, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:(3-5), exemplarily 1:3.5, 1:3.8, 1:4, 1:4.2 or 1:4.5, but not limited thereto. By adjusting the thickness ratio of the quantum well layer to the composite quantum barrier layer, the internal quantum efficiency of the product is improved.

[0039] More preferably, along the epitaxial growth direction, the thickness ratio of the quantum well layer and the composite quantum barrier layer in different sub-layers is reduced. Since the tunneling leakage current under low current density is the main reason for the decrease in IQE, the thickness of the quantum barrier layer of the main light-emitting well is thinned, the QCSE effect caused by internal piezoelectric polarization is reduced, and the thickness of the quantum barrier layer of the secondary light-emitting well is increased, the overall crystal quality is improved, the leakage channel is reduced, and the internal quantum efficiency of the product is improved.

[0040] In one embodiment, the N-type doping concentration of the composite quantum barrier layer is 1×10 17 cm -3 ~1×10 18 cm -3 , an exemplary value is 2.5×10 17 cm -3 , 3×10 17 cm -3 , 5×10 17 cm -3 , 7.5×10 17 cm -3 ,9×10 17 cm -3 , but not limited to this. In each composite quantum barrier layer, the first N-type GaN layer has the same N-type doping concentration as the N-type AlGaN layer, the second N-type GaN layer has the same N-type doping concentration as the N-type InGaN layer, and the ratio of the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer to the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is (2-5):1, exemplarily 2.5:1, 3:1, 3.5:1, 4:1 or 4.5:1, but not limited to this. Under low current density, the tunneling rate of carriers is greater than the rate of carrier recombination. A gradient N-type doping is set in the composite quantum barrier layer, so that the electrons moving into the quantum well are not easy to reverse tunnel, which promotes the movement of electrons to the P-type semiconductor side, while reducing the hole blocking barrier, improving the matching degree of electrons and holes, further improving the effective radiation recombination efficiency, and reducing the operating voltage.

[0041] Preferably, along the epitaxial growth direction, the N-type doping concentration of the composite quantum barrier layer in different sublayers decreases. Through the gradual change of the N-type doping concentration, the number of electrons ionized in the quantum well also gradually changes from more to less, which promotes the injection of holes into deeper quantum well layers to undergo radiation recombination with electrons under low current, and at the same time can shield the polarization electric field in the quantum well, increase the overlap of hole and electron wave functions, and increase the effective radiation recombination efficiency.

[0042] In addition to the above-mentioned multi-quantum well layer structure, the other layered structures of the present invention are characterized as follows:

[0043] The substrate 1 can be selected from one of sapphire substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate and zinc oxide substrate. Specifically, the substrate is selected from sapphire substrate, which is widely used in current LED production and has the advantages of mature preparation process, low price, good chemical stability and thermal stability.

[0044] The buffer layer 2 may be one or more of an AlN buffer layer, an AlGaN buffer layer, and a GaN buffer layer. Specifically, the buffer layer is an AlN buffer layer with a thickness of 10 nm to 30 nm.

[0045] The N-type semiconductor layer 3 may be an N-GaN layer with a thickness of 2 μm to 3 μm and a Si doping concentration of 1×10 19 cm -3 ~1×10 20 cm -3 .

[0046] The stress release layer 4 can be a Si-doped InGaN / GaN periodic alternating stacked structure, the number of periods is 5-8, the thickness of the InGaN layer in each period is 2nm-5nm, the thickness of the GaN layer is 5nm-10nm, and the Si doping concentration is 1×10 15 cm -3 ~1×10 17 cm -3 .

[0047] The P-type semiconductor layer 6 may be a P-GaN layer with a thickness of 50 nm to 80 nm and a Mg doping concentration of 1×10 15 cm -3 ~1×10 18 cm -3 .

[0048] Correspondingly, such as Figure 2 As shown, the present invention also provides a method for preparing an LED epitaxial wafer, comprising the following steps:

[0049] S1. providing a substrate;

[0050] In one embodiment, the substrate is a sapphire substrate.

[0051] S2, sequentially growing a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer on the substrate; the epitaxial structure can be grown by MOCVD, MBE, PVD or VPE, but is not limited thereto. Specifically, S2 includes the following steps:

[0052] S21, growth buffer layer;

[0053] The AlN buffer layer is grown by PVD. In one embodiment, the sapphire substrate coated with the AlN buffer layer is transferred to MOCVD and pretreated in H2 atmosphere for 1 min to 10 min at a temperature of 1000°C to 1200°C, which can improve the crystal quality of the AlN buffer layer and the crystal quality of the subsequently deposited GaN epitaxial layer.

[0054] S22, growing an N-type semiconductor layer;

[0055] The N-GaN layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 1000°C~1200°C, the pressure is 100Torr~600Torr, and N source, Ga source and N-type doping source are introduced.

[0056] S23, growing a stress release layer;

[0057] MOCVD is used to grow a Si-doped InGaN / GaN periodic alternating stacked structure, the reaction chamber temperature is controlled to be 800℃~900℃, the pressure is 100Torr~600Torr, N source, Ga source, In source and N-type doping source are introduced to grow an InGaN layer, N source, Ga source and N-type doping source are introduced to grow a GaN layer, and the InGaN layer and the GaN layer are repeatedly stacked to grow periodically.

[0058] S24, growing a multi-quantum well layer;

[0059] MOCVD growth is adopted to sequentially grow the first sublayer, the second sublayer to the Nth sublayer, and the growth method of each sublayer includes: controlling the temperature of the reaction chamber to 790℃~810℃, the pressure to 50Torr~300Torr, introducing N source, Ga source and In source, and growing the quantum well layer; controlling the temperature of the reaction chamber to 800℃~1000℃, the growth pressure to 50Torr~300Torr, and growing the composite quantum barrier layer; repeatedly stacking and periodically growing the quantum well layer and the composite quantum barrier layer. Specifically, the growth of the composite quantum barrier layer includes the following steps:

[0060] The temperature of the reaction chamber is controlled to be 800°C~1000°C, the growth pressure is 50Torr~300Torr, and N source, Ga source and N-type doping source are introduced to grow the first N-type GaN layer; N source, Ga source, Al source and N-type doping source are introduced to grow the N-type AlGaN layer; N source, Ga source and N-type doping source are introduced to grow the second N-type GaN layer; N source, Ga source, In source and N-type doping source are introduced to grow the N-type InGaN layer.

[0061] In different sub-layers, the growth temperature of the quantum well layer decreases first and then increases.

[0062] S25, growing a P-type semiconductor layer;

[0063] The P-GaN layer is grown by MOCVD, the temperature of the reaction chamber is controlled to be 800°C~980°C, the pressure is 100Torr~600Torr, and N source, Ga source and P-type doping source are introduced.

[0064] During the MOCVD growth process, the N source may be NH3, the Ga source may be TMGa and / or TEGa, the Al source may be TMAl, the In source may be TMIn, the N-type doping source may be SiH4, and the P-type doping source may be CP2Mg, but are not limited thereto.

[0065] The present invention will be further described below with specific embodiments:

[0066] Example 1

[0067] This embodiment provides an LED epitaxial wafer, including a substrate and a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer sequentially deposited on the substrate.

[0068] The multi-quantum well layer includes three sub-layers, each of which includes 10 periodically alternately stacked quantum well layers and composite quantum barrier layers. In each period, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:3.

[0069] The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer includes a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence. The N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is 1×10 17 cm -3 The N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is 1×10 18 cm -3 .

[0070] Accordingly, the growth of the multi-quantum well layer includes sequentially growing the first sublayer, the second sublayer and the third sublayer. The growth of the first sublayer, the second sublayer and the third sublayer each includes alternately growing InGaN quantum well layers and composite quantum barrier layers for 10 cycles.

[0071] The growth temperatures of the InGaN quantum well layers in the first sublayer, the second sublayer and the third sublayer are 803° C., 800° C. and 803° C. respectively.

[0072] Example 2

[0073] This embodiment provides an LED epitaxial wafer, which is different from the embodiment 1 in that the multi-quantum well layer includes 20 sub-layers, each of which includes a quantum well layer and a composite quantum barrier layer that are periodically alternately stacked. In each period, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:5.

[0074] The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer includes a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence. The N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is 1×10 17 cm -3 The N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is 5×10 17 cm -3 .

[0075] Accordingly, the growth of the multi-quantum well layer includes sequentially growing the first sublayer, the second sublayer, and the twentieth sublayer. The growth of each sublayer includes growing an InGaN quantum well layer and a composite quantum barrier layer.

[0076] The growth temperature of the sublayers was decreased from 795°C to 790°C and then increased to 795°C with a difference of 0.5°C per sublayer.

[0077] The rest are the same as in Example 1.

[0078] Example 3

[0079] This embodiment provides an LED epitaxial wafer, which is different from the embodiment 1 in that the multi-quantum well layer includes three sub-layers, each of which includes four periodically alternately stacked quantum well layers and composite quantum barrier layers. In each period, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:5.

[0080] The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer includes a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence. The N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is 2×10 17 cm -3The N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is 8×10 17 cm -3 .

[0081] Accordingly, the growth of the multi-quantum well layer includes sequentially growing the first sublayer, the second sublayer and the third sublayer. The growth of the first sublayer, the second sublayer and the third sublayer each includes four cycles of alternately growing InGaN quantum well layers and composite quantum barrier layers.

[0082] The growth temperatures of the InGaN quantum well layers in the first sublayer, the second sublayer and the third sublayer are 801° C., 800° C. and 801° C. respectively.

[0083] The rest are the same as in Example 1.

[0084] Example 4

[0085] This embodiment provides an LED epitaxial wafer, which is different from the embodiment 3 in that the thickness ratio of the quantum well layer and the composite quantum barrier layer in the first sublayer, the second sublayer and the third sublayer is reduced from 1:3 to 1:5. In the composite quantum barrier layer, the ratio of the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer to the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is reduced from 5:1 to 2:1.

[0086] The rest is the same as Example 3.

[0087] Example 5

[0088] This embodiment provides an LED epitaxial wafer, which differs from Embodiment 3 in that the growth rate of the composite quantum barrier layer in the first sublayer, the second sublayer and the third sublayer decreases from 0.035 nm / s to 0.02 nm / s.

[0089] The rest is the same as Example 3.

[0090] Comparative Example 1

[0091] This comparative example provides an LED epitaxial wafer, which is different from Example 1 in that the multi-quantum well layer includes periodically alternately stacked InGaN quantum well layers and GaN quantum barrier layers, with a period of 10. In each period, the thickness of the InGaN quantum well layer is 3.5nm, and the thickness of the GaN quantum barrier layer is 10nm. Accordingly, the preparation steps of the multi-quantum well layer are as follows: adopt MOCVD growth, control the reaction chamber temperature to 795°C, the pressure to 200Torr, introduce NH3 as the N source, N2 as the carrier gas, introduce TEGa as the Ga source, introduce TMIn as the In source, and grow the InGaN quantum well layer; control the reaction chamber temperature to 855°C, keep the pressure unchanged, introduce NH3 as the N source, N2 and H2 as the carrier gas, introduce TEGa as the Ga source, and grow the GaN quantum barrier layer; repeat the periodic growth of the InGaN quantum well layer and the GaN quantum barrier layer by stacking.

[0092] The rest are the same as in Example 1.

[0093] Comparative Example 2

[0094] This comparative example provides an LED epitaxial wafer, which differs from Example 1 in that the growth temperature of the quantum well layers in different sub-layers remains unchanged, and the growth temperature is 800°C.

[0095] The rest are the same as in Example 1.

[0096] The LED epitaxial wafers of Examples 1 to 5, Comparative Examples 1 and 2 were made into chips and heated at 60 mA (current density of about 12 A / cm 2 ) current, and calculated the improvement in light efficiency of Examples 1 to 5 and Comparative Example 2 compared with Comparative Example 1. The specific results are as follows:

[0097]

[0098] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. An LED epitaxial wafer, It is characterized in that It includes a substrate and a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer sequentially deposited on the substrate, wherein the multi-quantum well layer includes at least three sublayers, and each sublayer includes a quantum well layer and a composite quantum barrier layer that are periodically and alternately stacked; The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer comprises a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence; the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer; Along the epitaxial growth direction, the growth temperature of the quantum well layer in different sub-layers first decreases and then increases, and the growth rate of the composite quantum barrier layer in different sub-layers decreases.

2. The LED epitaxial wafer according to claim 1, It is characterized in that The number of sublayers of the multi-quantum well layer is 3 to 20, and each sublayer includes a periodic structure in which 1 to 10 quantum well layers and composite quantum barrier layers are alternately grown.

3. The LED epitaxial wafer according to claim 1, It is characterized in that The thickness of the multi-quantum well layer is 100nm-300nm; in each period of each sub-layer, the thickness ratio of the quantum well layer to the composite quantum barrier layer is 1:(3-5).

4. The LED epitaxial wafer according to claim 1, It is characterized in that The N-type doping concentration of the composite quantum barrier layer is 1×10 17 cm -3 ~1×10 18 cm -3 ; In each composite quantum barrier layer, the N-type doping concentration of the first N-type GaN layer is the same as that of the N-type AlGaN layer, the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is the same, and the ratio of the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer to the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer is (2~5):

1.

5. The LED epitaxial wafer according to claim 3, It is characterized in that Along the epitaxial growth direction, the thickness ratio of the quantum well layer and the composite quantum barrier layer in different sub-layers decreases.

6. The LED epitaxial wafer according to claim 1, It is characterized in that The difference in growth temperature of the quantum well layer of two adjacent sub-layers is 0.5°C to 3°C.

7. The LED epitaxial wafer according to claim 1, It is characterized in that Along the epitaxial growth direction, the growth rate of the composite quantum barrier layer in different sub-layers decreases.

8. A method for preparing an LED epitaxial wafer, for preparing the LED epitaxial wafer as claimed in any one of claims 1 to 7, It is characterized in that The following steps are involved: A substrate is provided, and a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well layer and a P-type semiconductor layer are sequentially grown on the substrate, wherein the multi-quantum well layer includes at least three sublayers, and each sublayer includes a quantum well layer and a composite quantum barrier layer that are periodically and alternately stacked; The quantum well layer is an InGaN quantum well layer, and the composite quantum barrier layer comprises a first N-type GaN layer, an N-type AlGaN layer, a second N-type GaN layer and an N-type InGaN layer stacked in sequence; the N-type doping concentration of the second N-type GaN layer and the N-type InGaN layer is greater than the N-type doping concentration of the first N-type GaN layer and the N-type AlGaN layer; Along the epitaxial growth direction, the growth temperature of the quantum well layer in different sub-layers first decreases and then increases.

9. The method for preparing an LED epitaxial wafer according to claim 8, It is characterized in that The growth temperature of the quantum well layer is 790° C. to 810° C., and the growth pressure is 50 Torr to 300 Torr; The growth temperature of the composite quantum barrier layer is 800° C. to 1000° C., and the growth pressure is 50 Torr to 300 Torr.

10. An LED, It is characterized in that The LED comprises the LED epitaxial wafer as claimed in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Epitaxial growth method for improving brightness of light-emitting diode based on active layer

    CN105932126A

  • Manufacturing method for epitaxial wafer of GaN-based light-emitting diode

    CN106057989A