High-performance anhydrous gun clay and its preparation method

Through scientific proportioning and advanced processes of raw materials such as high alumina bauxite, high-performance waterless gun mud was prepared, which solved the problems of unstable quality and insufficient corrosion resistance of existing waterless gun mud, and achieved high strength and slag resistance , the improvement of anti-iron erosion and anti-shrink performance extends the iron production time and reduces production costs.

CN118530011BActive Publication Date: 2024-11-12ULANQAB CITY XIMENDING NEW TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010773.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In actual application of existing waterless cannon mud, there are problems such as unstable product quality, difficulty in maintaining the depth of the iron mouth, insufficient corrosion resistance, etc., resulting in short iron production time, insufficient iron production volume, frequent iron leakage, and increased Production costs and reduced production efficiency.

Method used

Using scientific proportions of raw materials such as high-alumina bauxite, electromelting mullite, silicon carbide, boron nitride, hafnium oxide, graphite, silicon sol, polyborosiloxane, titanium carbide whiskers and nano ceria, and Through dry ball milling, stirring, ultrasonic dispersion and heat treatment, high-performance water-free cannon mud is prepared to improve its strength, slag resistance, molten iron erosion and erosion resistance.

Benefits of technology

Improve the strength and stability of waterless cannon mud, enhance the resistance to slag, iron erosion and erosion resistance, extend the iron discharge time, reduce the phenomenon of iron seepage, iron leakage, reduce production costs, and meet the blast furnace reinforced smelting need.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-performance anhydrous cannon clay and a preparation method thereof. The cannon clay comprises, by weight, 38-48 parts of high-alumina bauxite, 18-23 parts of fused mullite, 10-14 parts of silicon carbide, 4-6 parts of boron nitride, 0.5-1 parts of hafnium oxide, 3-4 parts of graphite, 6-8 parts of silica sol, 2-3 parts of polyborosiloxane, 0.3-0.5 parts of titanium carbide whiskers, 0.1-0.3 parts of nano cerium dioxide and 1-2 parts of magnesium oxide. The preparation method includes: first, mixing high-alumina bauxite, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide in a specified proportion; then, stirring and mixing silica sol and polyborosiloxane at 75-85°C for 2 hours, adding nano-cerium dioxide after cooling to room temperature; then, mixing the dry ball-milled powder material with the mixed liquid binder and titanium carbide whiskers, and stirring in a vacuum mixer for 30-60 minutes; finally, isostatically pressing the mixture at a pressure of 20-25MPa to obtain the final product. The taphole mud has the advantages of high strength, good volume stability, and strong slag resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to high-performance anhydrous taphole mud and a preparation method thereof. Background Art

[0002] With the continuous advancement of blast furnace smelting technology, the requirements for blast furnace taphole work are becoming more and more stringent. In order to maintain the stability of the taphole working state and meet the needs of efficient smelting in the blast furnace, it is usually necessary to use taphole mud to seal the taphole to protect the furnace wall and furnace bottom in the taphole area. This requires that the taphole mud has excellent operating performance to ensure that the taphole is fully filled; it has good volume stability and can be sintered quickly; it has the ability to dry and harden quickly and maintain high strength at high temperatures; in addition, the taphole mud also needs to have good opening performance, be easy to reopen, and be able to resist slag iron erosion, scouring and oxidation.

[0003] Traditional blast furnace taphole mud is mainly divided into two categories: water-containing taphole mud and water-free taphole mud. Water-containing taphole mud is mainly made of raw materials such as coke powder, clay, fuel, water and asphalt. Although it has a low cost, its strength is poor and its resistance to slag, molten iron erosion and scouring is weak. In contrast, water-free taphole mud is made of corundum, silicon carbide, coke powder, clay and various binders as the main raw materials. Because it does not contain water, it has higher strength and better resistance to slag, molten iron erosion and scouring, so it has gradually become the mainstream.

[0004] However, the existing anhydrous taphole mud still has some problems in practical application, such as unstable product quality, difficult taphole depth maintenance, insufficient corrosion resistance, etc. These problems will lead to short tapping time, insufficient tapping volume, frequent iron seepage and leakage, which will increase production costs and reduce the production efficiency and profitability of enterprises. Summary of the invention

[0005] The present application provides a high-performance anhydrous taphole mud with high strength, good stability, excellent slag resistance, resistance to molten iron erosion and scouring resistance, so as to meet the needs of blast furnace intensive smelting, improve iron tapping time and iron tapping amount, reduce iron seepage and leakage, and reduce product costs.

[0006] The high-performance anhydrous cannon mud provided by the present application includes the following components by weight: 38-48 parts of high-alumina bauxite, 18-23 parts of fused mullite, 10-14 parts of silicon carbide, 4-6 parts of boron nitride, 0.5-1 parts of hafnium oxide, 3-4 parts of graphite, 6-8 parts of silica sol, 2-3 parts of polyborosiloxane, 0.3-0.5 parts of titanium carbide whiskers, 0.1-0.3 parts of nano-cerium dioxide, and 1-2 parts of magnesium oxide.

[0007] Furthermore, in the present application, the Al2O3 content of the high-alumina bauxite is ≥95%, and the particle size is 1-3mm; the Al2O3 content of the fused mullite is ≥75%, and the particle size is 0-1mm; the purity of silicon carbide is ≥98%, and the particle size is ≤45μm; the boron nitride is hexagonal boron nitride, with a purity of ≥99% and a particle size of ≤45μm; the graphite is flake graphite, with a purity of ≥99% and a particle size of ≤45μm; the SiO2 content in the silica sol is 30-35%, and the particle size is 10-20nm; the boron content in the polyborosiloxane is 10-15%, and the molecular weight is 1000-10000; the diameter of the titanium carbide whisker is 0.5-2μm, and the length is 20-100μm; the particle size of nano-cerium dioxide is ≤50nm, and the specific surface area is ≥30 m² / g; the purity of magnesium oxide is ≥98%, and the particle size is ≤75μm.

[0008] The preparation method of anhydrous cannon mud provided in the present application comprises the following steps: first, high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide are mixed in proportion, and dry-milled in a planetary ball mill for 4-6 hours; then, silica sol and polyborosiloxane are stirred and mixed at 75-85°C for 2 hours, and nano-cerium dioxide is added after cooling to room temperature, and ultrasonically dispersed for 30 minutes; then, the powder material is mixed with a liquid binder and titanium carbide whiskers, and stirred in a vacuum mixer for 30-60 minutes; finally, the mixture is isostatically pressed at a pressure of 20-25MPa, and heat-treated under argon protection: first, it is kept at 200°C for 2 hours, then raised to 350°C for 4 hours, and finally cooled to room temperature to obtain the final product.

[0009] In the present application, high-alumina bauxite provides a high content of Al2O3, which significantly improves the refractory performance and high-temperature strength, ensuring that the anhydrous cannon mud remains structurally stable at high temperatures. Fused mullite enhances the thermal stability and thermal shock resistance of the material, and reduces the stress caused by thermal expansion and contraction. Silicon carbide has extremely high wear resistance and thermal conductivity, reduces thermal expansion differences, and enhances volume stability and crack resistance. Graphite provides good thermal conductivity and lubricity, further improving the thermal shock resistance and crack resistance of the material. Boron nitride has high chemical corrosion resistance, especially at high temperatures, and can effectively resist chemical corrosion of slag iron. Titanium carbide whiskers improve the durability of cannon mud under high-temperature molten iron scouring by enhancing mechanical strength and wear resistance. Magnesium oxide provides basic refractory performance and chemical corrosion resistance, further improving the corrosion resistance of the material. Nano-cerium dioxide enhances oxidation resistance, prevents oxidative degradation at high temperatures, and extends the service life of anhydrous cannon mud, thereby increasing the iron-out time and iron-out amount. Silica sol and polyborosiloxane as binders provide good adhesion and toughness, ensuring the stability and consistency of the material during processing, while improving the opening performance of the taphole mud, making it easier to machine and use. Hafnium oxide provides additional strength and stability at high temperatures, ensuring consistent performance of the taphole mud in practical applications.

[0010] The anhydrous taphole mud prepared by the present application through scientific proportioning of multiple raw materials and advanced preparation technology has the following advantages: high strength and high temperature stability, which can effectively protect the iron mouth area of ​​the blast furnace; good volume stability and crack resistance, ensuring long-term use in high temperature environment; excellent resistance to slag erosion and scouring, extending the iron-out time and increasing the iron-out amount; good processing and opening performance, reducing production costs. DETAILED DESCRIPTION

[0011] Many specific details are described in the following description to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present application, so the present application is not limited by the specific implementation disclosed below.

[0012] Embodiment 1:

[0013] Weigh the following raw materials in parts by weight: 48 parts of high-alumina bauxite (including Al2O3 content ≥95%, particle size 1-3mm), 23 parts of fused mullite (including Al2O3 content ≥75%, particle size 0-1mm), 14 parts of silicon carbide (purity ≥98%, particle size ≤45μm), 6 parts of boron nitride (specifically hexagonal boron nitride, purity ≥99%, particle size ≤45μm), 1 part of hafnium oxide (purity ≥99%), graphite 4 parts (specifically flake graphite, purity ≥99%, particle size ≤45μm), 8 parts of silica sol (SiO2 content 30-35%, particle size 10-20nm), 3 parts of polyborosiloxane (boron content 10-15%, molecular weight 1000-10000), 0.5 parts of titanium carbide whiskers (diameter 0.5-2μm, length 20-100μm), 0.3 parts of nano cerium dioxide (particle size ≤50nm, specific surface area ≥30 m² / g), 2 parts of magnesium oxide (purity ≥98%, particle size ≤75μm).

[0014] The preparation method is as follows:

[0015] S1: high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide are mixed according to the above weight proportions, and dry-milled in a planetary ball mill for 6 hours to obtain a uniform powder mixture.

[0016] S2: Silica sol and polyborosiloxane were stirred and mixed at 85° C. for 2 hours according to the above weight proportions, and nano-cerium dioxide was added after cooling to room temperature, and ultrasonically dispersed for 30 minutes to obtain a uniform liquid mixture.

[0017] S3: Mix the powder material obtained in step S1 with the liquid binder in step S2, add titanium carbide whiskers, and stir in a vacuum mixer for 60 minutes to ensure that all ingredients are evenly distributed.

[0018] S4: The mixture is isostatically pressed at a pressure of 25 MPa to obtain a preliminarily formed cannon clay body.

[0019] S5: The formed cannon clay body is heat treated under argon protection: first, it is kept at 200°C for 2 hours, then the temperature is increased to 350°C and kept for 4 hours, and then slowly cooled to room temperature to obtain the final high-performance anhydrous cannon clay.

[0020] Embodiment 2:

[0021] Weigh the following raw materials in parts by weight: 38 parts of high-alumina bauxite (wherein, Al2O3 content ≥95%, particle size 1-3mm), 18 parts of fused mullite (Al2O3 content ≥75%, particle size 0-1mm), 10 parts of silicon carbide (purity ≥98%, particle size ≤45μm), 4 parts of boron nitride (specifically hexagonal boron nitride, purity ≥99%, particle size ≤45μm), 0.5 parts of hafnium oxide (purity ≥99%), stone 3 parts of ink (flake graphite, purity ≥99%, particle size ≤45μm), 6 parts of silica sol (SiO2 content 30-35%, particle size 10-20nm), 2 parts of polyborosiloxane (boron content 10-15%, molecular weight 1000-10000), 0.3 parts of titanium carbide whiskers (diameter 0.5-2μm, length 20-100μm), 0.1 parts of nano cerium dioxide (particle size ≤50nm, specific surface area ≥30 m² / g), 1 part of magnesium oxide (purity ≥98%, particle size ≤75μm).

[0022] The preparation method is as follows:

[0023] S1: high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide are mixed according to the above weight proportions, and dry-milled in a planetary ball mill for 6 hours to obtain a uniform powder mixture.

[0024] S2: Silica sol and polyborosiloxane were stirred and mixed at 85° C. for 2 hours according to the above weight proportions, and nano-cerium dioxide was added after cooling to room temperature, and ultrasonically dispersed for 30 minutes to obtain a uniform liquid mixture.

[0025] S3: Mix the powder material obtained in step S1 with the liquid binder in step S2, add titanium carbide whiskers, and stir in a vacuum mixer for 60 minutes to ensure that all ingredients are evenly distributed.

[0026] S4: The mixture is isostatically pressed at a pressure of 25 MPa to obtain a preliminarily formed cannon clay body.

[0027] S5: The formed cannon clay body is heat treated under argon protection: first, it is kept at 200°C for 2 hours, then the temperature is increased to 350°C and kept for 4 hours, and then slowly cooled to room temperature to obtain the final high-performance anhydrous cannon clay.

[0028] Embodiment 3:

[0029] Weigh the following raw materials in parts by weight: 40 parts of high-alumina bauxite (Al2O3 content ≥95%, particle size 1-3mm), 19 parts of fused mullite (Al2O3 content ≥75%, particle size 0-1mm), 11 parts of silicon carbide (purity ≥98%, particle size ≤45μm), 5 parts of boron nitride (hexagonal boron nitride, purity ≥99%, particle size ≤45μm), 0.7 parts of hafnium oxide (purity ≥99%), 3.5 parts of graphite (flake graphite, purity ≥99%, particle size ≤45μm), silica sol 7 parts (SiO2 content 30-35%, particle size 10-20nm), polyborosiloxane 2.5 parts (B content 10-15%, molecular weight 1000-10000), titanium carbide whisker 0.4 parts (diameter 0.5-2μm, length 20-100μm), nano cerium dioxide 0.2 parts (particle size ≤50nm, specific surface area ≥30 m² / g), magnesium oxide 1.5 parts (purity ≥98%, particle size ≤75μm).

[0030] The preparation method is as follows:

[0031] S1: high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide are mixed according to the above weight proportions, and dry-milled in a planetary ball mill for 6 hours to obtain a uniform powder mixture.

[0032] S2: Silica sol and polyborosiloxane were stirred and mixed at 85° C. for 2 hours according to the above weight proportions, and nano-cerium dioxide was added after cooling to room temperature, and ultrasonically dispersed for 30 minutes to obtain a uniform liquid mixture.

[0033] S3: Mix the powder material obtained in step S1 with the liquid binder in step S2, add titanium carbide whiskers, and stir in a vacuum mixer for 60 minutes to ensure that all ingredients are evenly distributed.

[0034] S4: The mixture is isostatically pressed at a pressure of 25 MPa to obtain a preliminarily formed cannon clay body.

[0035] S5: The formed cannon clay body is heat treated under argon protection: first, it is kept at 200°C for 2 hours, then the temperature is increased to 350°C and kept for 4 hours, and then slowly cooled to room temperature to obtain the final high-performance anhydrous cannon clay.

[0036] Embodiment 4:

[0037] Weigh the following raw materials in parts by weight: 42 parts of high-alumina bauxite (Al2O3 content ≥95%, particle size 1-3mm), 20 parts of fused mullite (Al2O3 content ≥75%, particle size 0-1mm), 12 parts of silicon carbide (purity ≥98%, particle size ≤45μm), 4.5 parts of boron nitride (hexagonal boron nitride, purity ≥99%, particle size ≤45μm), 0.8 parts of hafnium oxide (purity ≥99%), 3.2 parts of graphite ( Flake graphite, purity ≥99%, particle size ≤45μm), 6.5 parts of silica sol (SiO2 content 30-35%, particle size 10-20nm), 2.2 parts of polyborosiloxane (boron content 10-15%, molecular weight 1000-10000), 0.35 parts of titanium carbide whiskers (diameter 0.5-2μm, length 20-100μm), 0.15 parts of nano cerium dioxide (particle size ≤50nm, specific surface area ≥30 m² / g), 1.2 parts of magnesium oxide (purity ≥98%, particle size ≤75μm).

[0038] The preparation method is as follows:

[0039] S1: high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide are mixed according to the above weight proportions, and dry-milled in a planetary ball mill for 6 hours to obtain a uniform powder mixture.

[0040] S2: Silica sol and polyborosiloxane were stirred and mixed at 85° C. for 2 hours according to the above weight proportions, and nano-cerium dioxide was added after cooling to room temperature, and ultrasonically dispersed for 30 minutes to obtain a uniform liquid mixture.

[0041] S3: Mix the powder material obtained in step S1 with the liquid binder in step S2, add titanium carbide whiskers, and stir in a vacuum mixer for 60 minutes to ensure that all ingredients are evenly distributed.

[0042] S4: The mixture is isostatically pressed at a pressure of 25 MPa to obtain a preliminarily formed cannon clay body.

[0043] S5: The formed cannon clay body is heat treated under argon protection: first, it is kept at 200°C for 2 hours, then the temperature is increased to 350°C and kept for 4 hours, and then slowly cooled to room temperature to obtain the final high-performance anhydrous cannon clay.

[0044] According to the test steps shown in GB / T16555, YB / T5200, GB / T5988 and GB / T5072, the performance of the prepared anhydrous taphole mud was measured. The test results are shown in Table 1 below:

[0045] Table 1. Comparison of performance tests of anhydrous taphole mud

[0046] ;

[0047] The test results show that the anhydrous taphole clays prepared in different embodiments all have high bulk density, good compressive strength at room temperature and small permanent line change upon heating, indicating that the anhydrous taphole clay of the present invention has excellent performance in a high-temperature smelting environment and can meet the needs of blast furnace intensive smelting.

[0048] Although the present application is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present application. Any technical personnel in this field may make possible changes and modifications without departing from the spirit and scope of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A high performance anhydrous taphole mud, characterized in that: By weight, it includes the following components: 38-48 parts of high alumina; 18-23 parts of fused mullite; Silicon carbide 10-14 parts; Boron nitride 4-6 parts; Hafnium oxide 0.5-1 part; 3-4 parts of graphite; 6-8 parts of silica sol; 2-3 parts of polyborosiloxane; Titanium carbide whisker 0.3-0.5 parts; Nano cerium dioxide 0.1-0.3 parts; 1-2 parts of magnesium oxide.

2. The high performance anhydrous taphole mud according to claim 1, characterized in that: The Al2O3 content of the high-alumina bauxite is ≥95%, and the particle size is 1-3mm.

3. The high performance anhydrous taphole mud according to claim 1, characterized in that: The Al2O3 content of the fused mullite is ≥75%, and the particle size is 0-1mm.

4. The high performance anhydrous taphole mud according to claim 1, characterized in that: The purity of the silicon carbide is ≥98% and the particle size is ≤45 μm.

5. The high performance anhydrous taphole mud according to claim 1, characterized in that: The boron nitride is hexagonal boron nitride with a purity of ≥99% and a particle size of ≤45 μm.

6. The high performance anhydrous taphole mud according to claim 1, characterized in that: The graphite is flake graphite with a purity of ≥99% and a particle size of ≤45 μm.

7. The high performance anhydrous taphole mud according to claim 1, characterized in that: The SiO2 content in the silica sol is 30-35%, and the particle size is 10-20nm.

8. The high performance anhydrous taphole mud according to claim 1, characterized in that: The B content in the polyborosiloxane is 10-15%, and the molecular weight is 1000-10000.

9. The high performance anhydrous taphole mud according to claim 1, characterized in that: The diameter of the titanium carbide whisker is 0.5-2 μm, and the length is 20-100 μm; the particle size of the nano-cerium dioxide is ≤50 nm, and the specific surface area is ≥30 m² / g; the purity of the magnesium oxide is ≥98%, and the particle size is ≤75 μm.

10. A method for preparing high-performance anhydrous taphole mud as claimed in claim 1, characterized in that: The following steps are involved: S1: mixing high alumina, fused mullite, silicon carbide, boron nitride, hafnium oxide, graphite and magnesium oxide according to the weight percentage specified in claim 1, and dry-milling them in a planetary ball mill for 4-6 hours; S2: According to the weight percentage specified in claim 1, silica sol and polyborosiloxane are stirred and mixed at 75-85° C. for 2 hours, and after cooling to room temperature, nano-cerium dioxide is added and ultrasonically dispersed for 30 minutes; S3: mixing the powder material of step S1 with the liquid binder of step S2, adding titanium carbide whiskers according to the weight percentage specified in claim 1, and stirring in a vacuum mixer for 30-60 minutes; S4: isostatically pressing the mixture at a pressure of 20-25 MPa; S5: The formed taphole clay is heat treated under argon protection using the following heating method: first keep it at 200°C for 2 hours, then increase the temperature to 350°C and keep it for 4 hours, and finally cool it to room temperature to obtain the final product.