A method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox
Through atomization and cold spraying, lead-containing tin bronze alloy powder is evenly covered on the substrate. Combined with the laser cladding process, the problem of insufficient bearing performance and anti-blocking performance of sliding bearings in wind power gearboxes is solved, and the bearing material is realized Improved compliance and anti-ostealing properties.
Patent Information
- Application Number
- CN202411013404.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing sliding bearings have problems with insufficient bearing performance and anti-blocking performance in wind power gearboxes, especially the segregation phenomenon of lead-containing copper alloys by laser cladding process leads to uneven distribution, affecting the bearing compliance and anti-blocking properties.
The lead-containing tin bronze alloy powder is used to form small metal droplets, and it is uniformly covered on the substrate through cold spraying process. Then it is melted using laser cladding process to avoid segregation of lead at high temperatures, ensuring the compliance of bearing materials and Anti-osteal.
It improves the compliance and anti-bite properties of bearing materials, ensures the uniform distribution of lead, avoids segregation during laser cladding, and improves the overall performance of the bearing.
Smart Images

Figure CN118531387B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sliding bearings, and in particular to a method for preparing a lead-containing copper alloy sliding bearing for a wind power gear box. Background Art
[0002] Wind power generation is gradually becoming larger, and the bearings of wind power gearboxes are also getting larger. In order to reduce costs and solve the difficulties in the manufacturing process of large rolling bearings, it has become a trend to replace rolling bearings with sliding bearings. Sliding bearings can not only reduce the size of the gearbox, thereby making it lighter, but also increase the power density. That is, when using sliding bearings, they are smaller than rolling bearings, which can further reduce the size of the gearbox. Therefore, under the premise of unchanged power, the power density is improved.
[0003] However, wind power operating conditions are complex. During hoisting, start and stop, swing before grid connection, and insufficient oil supply, the lubrication state is in boundary lubrication. At this time, the lubrication performance of the material itself will play a key role.
[0004] At present, the most mature application of sliding bearings is the bushing made of low hardness materials such as MiBa tin-aluminum alloy. Although MiBa tin-aluminum alloy has good compliance and anti-bite properties, its load-bearing performance and wear resistance are poor. In order to improve the load-bearing performance, high-hardness tin bronze or aluminum bronze is usually used, and its preparation can also be laser cladding, but the anti-bite performance of this type of material is very poor. Therefore, lead-containing copper alloy can be used because it has good load-bearing performance, anti-bite performance and compliance. However, it is not very suitable for the laser cladding process.
[0005] Laser cladding technology is the mainstream technology of main engine manufacturers and gearbox manufacturers due to its advantages such as low cost, less materials and small bearing size. However, there are great problems in using laser cladding technology for lead-containing materials. For example, due to the high temperature of laser cladding and the high melting degree of copper alloy, while lead has a low melting point and high density, it is easy to cause serious segregation and the cladding quality is very poor. Summary of the invention
[0006] In view of this, the present invention provides a method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox to solve the above problems.
[0007] A method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox comprises the following steps:
[0008] STEP 101: Provide a substrate and place the substrate horizontally;
[0009] STEP102: sandblasting the substrate;
[0010] STEP 103: Provide a raw material of lead-tin bronze alloy powder, and provide an atomizing device to prepare uniformly distributed spherical lead-tin bronze alloy powder, wherein the raw material of the lead-tin bronze alloy powder is composed of Cu, Sn, and Pb, wherein the percentage of Sn in the raw material of the lead-tin bronze alloy powder is 2-15%, the percentage of Pb is 2-24%, and the rest is copper;
[0011] STEP 104: Spraying lead-tin bronze powder onto the substrate by cold spraying;
[0012] STEP 105: Use laser heating to heat the lead-tin bronze powder to a super solid phase sintering temperature of 750-900°C, so that the lead-tin bronze powder and the matrix are metallurgically bonded, and the bonding force reaches more than 200 MPa to complete the preparation of the lead-containing copper alloy sliding bearing.
[0013] Furthermore, the substrate is one of a copper shaft and an alloy shaft.
[0014] Furthermore, in step STEP102, during the sandblasting process, the substrate surface is sandblasted to remove oil stains and oxide scale on the substrate surface and to roughen the substrate, and the output pressure of the sandblasting equipment is 0.3 MPa.
[0015] Furthermore, the sand used in the sandblasting process is one of brown corundum, white corundum and pomegranate sand.
[0016] Furthermore, in step STEP103, the particle size of the prepared lead-tin bronze alloy powder is 10-150 um.
[0017] Furthermore, in step STEP 105, the equipment used for the laser heating method is a laser cladding machine.
[0018] Furthermore, the laser cladding machine is carried out along the axial direction of the substrate, and after heating to the end, the substrate is rotated by a certain angle to continue heating along the axial direction until the entire substrate is completely heated.
[0019] Furthermore, the equipment used for the laser heating is a laser cladding machine, the power of which is between 1000 and 5000 W, and the line speed is between 600 and 1800 mm / min.
[0020] Furthermore, the raw materials of the lead-tin bronze alloy powder include 74% copper, 4% tin, and 22% lead.
[0021] Further, in STEP 103, the raw material of the lead-tin bronze alloy powder is put into a high-frequency induction melting furnace for vacuum melting, wherein the vacuum degree is set to 6 Pa, the protective gas is argon, the induction power is set to 20 kW, and the induction time is set to 20 min to obtain a molten mixture.
[0022] Compared with the prior art, the preparation method of the lead-containing copper alloy sliding bearing for the wind power gearbox provided by the present invention adopts the lead-containing copper alloy, while ensuring the load-bearing capacity, it also takes into account the compliance and anti-bite property. Specifically, due to the presence of lead, the lubricity of the bearing material is improved, which is conducive to improving the compliance and anti-bite property of the bearing material. However, due to the presence of lead, higher requirements are placed on its preparation method, especially using the laser cladding process. Specifically, due to the high temperature of the laser cladding process, if the lead-containing copper alloy powder is directly clad on the substrate, it will not only aggregate but also segregate. In the present preparation method, the lead-containing copper alloy is formed into small metal droplets by an atomization process, and then the lead-containing tin bronze powder is sprayed on the substrate by cold spraying, so that the lead can be evenly covered on the substrate, and finally the lead-containing tin bronze layer is melted by the laser cladding process, which can prevent the lead from segregating at high temperature, thereby causing uneven distribution, so that the compliance and anti-bite property of the obtained bearing material can be guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention provides a flow chart of a method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox.
[0024] Figure 2 for Figure 1 Metallographic diagram of the lead-containing copper alloy material prepared by the preparation method of the lead-containing copper alloy sliding bearing for the wind power gear box.
[0025] Figure 3 This is a metallographic diagram of a lead-containing copper alloy material prepared by the preparation method of the comparative example. DETAILED DESCRIPTION
[0026] The specific embodiments of the present invention are further described in detail below. It should be understood that the description of the embodiments of the present invention herein is not intended to limit the protection scope of the present invention.
[0027] The present invention provides a method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox, which comprises the following steps:
[0028] STEP 101: Provide a substrate and place the substrate horizontally;
[0029] STEP 102: sandblasting the substrate.
[0030] STEP 103: Provide a raw material of lead-tin bronze alloy powder, and provide an atomizing device to prepare uniformly distributed spherical lead-tin bronze alloy powder, wherein the raw material of the lead-tin bronze alloy powder is composed of Cu, Sn, and Pb, wherein the percentage of Sn in the raw material of the lead-tin bronze alloy powder is 2-15%, the percentage of Pb is 2-24%, and the rest is copper;
[0031] STEP 104: Spraying lead-tin bronze powder onto the substrate by cold spraying;
[0032] STEP 105: Use laser heating to heat the lead-tin bronze powder to an instantaneous liquid-solid sintering temperature between 750-900°C, so that the lead-tin bronze powder and the matrix are metallurgically bonded, and the bonding force reaches more than 200 MPa to complete the preparation of the lead-containing copper alloy sliding bearing.
[0033] In step STEP101, the substrate may be a steel shaft, a copper shaft, an alloy shaft, or a stainless steel shaft.
[0034] In step STEP102, the sandblasting process itself is a prior art, which uses compressed air to spray sand onto the surface of the substrate, thereby removing oil stains and oxide scale on the surface and making the substrate rough, thereby improving the bonding strength after cladding in the subsequent process. In this embodiment, the sandblasting process can use the preparation method in the prior art.
[0035] In step STEP103, the atomization process itself is also a prior art, and its core principle is to use high-pressure air flow or water flow, centrifugal force or vacuum decompression to crush the molten metal liquid flow into droplets of fine particle size, and obtain metal or alloy powder after condensation. When the metal is melted, the metal is placed in a vacuum high-frequency induction furnace, that is, when atomizing and powdering, different metals are first melted in the induction furnace, and then the alloy liquid is blown away by gas and cooled into copper alloy powder. The atomization process has low cost, high efficiency and good performance, so it is better than the general grinding process. In this embodiment, the raw materials of the lead-tin bronze alloy powder are composed of Cu, Sn and Pb. In the raw materials of the lead-tin bronze alloy powder, the lead content is set between 2% and 24%. If the lead content is lower than 2%, the lubricity is insufficient, and if the lead content is higher than 24%, the material strength will be affected. The tin content is set between 2% and 15%. If the tin content is less than 2%, it will not have a strengthening effect, while if the tin content is higher than 15%, the strength will decrease because the entire material will become brittle. When the content of lead and tin is determined, the remaining is copper.
[0036] The particle size of the produced lead-tin bronze alloy powder is 10-150um, which is the requirement of the cold spraying process. Particle sizes smaller than 10um or larger than 150um will result in poor spraying effects.
[0037] In step STEP104, the cold spraying process itself is a prior art, which is also called gas-powered spraying technology. It is a method in which a coating is formed by deposition after strong plastic deformation of high-speed solid particles with a certain plasticity collide with the substrate. Under normal conditions, the general concept is that when solid particles collide with a certain substrate, the solid particles will have an erosion effect on the substrate. The cold spraying process does not require the sprayed metal particles to be melted. It uses compressed air to accelerate the metal particles to a critical speed. After being sprayed, the metal particles are physically deformed after hitting the surface of the substrate. The metal particles are flattened on the surface of the substrate and firmly attached. The metal particles are not melted during the whole process. The lead-tin bronze alloy powder is attached to the substrate by the cold spraying process. Since the copper alloy contains lead, and the temperature of cold spraying is low, the oxidation of lead can be avoided by cold spraying, and the segregation of lead can also be avoided.
[0038] In step STEP105, the laser heating, also known as laser cladding, is a prior art. In this embodiment, the laser heating device is a laser cladding machine, whose power is between 1000 and 5000 W and whose line speed is between 600 and 1800 mm / min. Specifically, the substrate is placed horizontally, and the laser cladding machine is operated axially. After heating to the end, the substrate is rotated at a certain angle to continue axial heating until the entire substrate is heated. Example
[0039] A method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox comprises the following steps:
[0040] Step STEP101: providing a substrate and placing the substrate horizontally, wherein the substrate is made of a 42CrMo alloy material;
[0041] Step STEP102: using a sandblasting device to spray white corundum sand onto the surface of the substrate to remove oil stains and oxide scale on the surface of the substrate and make the substrate rough, the output pressure of the sandblasting device being 0.3 MPa;
[0042] Step STEP103: providing a raw material of lead-tin bronze alloy powder, which includes 80% copper, 10% tin, and 10% lead, and performing vacuum high-frequency induction melting on the raw material of lead-tin bronze alloy powder to obtain a molten mixture. Specifically, the raw material of lead-tin bronze alloy powder is put into a high-frequency induction melting furnace for vacuum melting, wherein the vacuum degree is set to 6 Pa, the protective gas is argon, the induction power is set to 20 kW, and the induction time is set to 20 min to obtain the molten mixture;
[0043] Step STEP104: After the smelting mixture is completely alloyed, the melt temperature is adjusted to 1200°C, and then the mixture is put into an atomizing device and atomized with argon gas to prepare powder. The vacuum atomizing process conditions include selecting high-purity argon gas as the protective gas, the vacuum degree is 5×104Pa, and the atomizing pressure is 3.5-3.6MPa. The lead-tin bronze alloy powder is subjected to particle size screening and powder drying, and then vacuum packaged to obtain the lead-tin bronze alloy powder. green Copper alloy powder;
[0044] Step STEP105: using cold spraying technology to spray lead-tin bronze alloy powder onto the surface of the substrate, with a thickness of 1 to 3 mm and a bonding force of 10 to 200 MPa;
[0045] Step STEP106: Use a laser cladding machine to heat the lead-tin bronze alloy powder to a target temperature of 820°C until the copper layer on the surface of the entire substrate is heated to achieve metallurgical bonding with a bonding force of 200 MPa, a laser power of 3000 W, and a line speed of 600 mm / min. Example
[0046] A method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox comprises the following steps:
[0047] Step STEP101: providing a substrate and placing the substrate horizontally, wherein the substrate is made of a 42CrMo alloy material;
[0048] Step STEP102: using a sandblasting device to spray white corundum sand onto the surface of the substrate to remove oil stains and oxide scale on the surface of the substrate and make the substrate rough, the output pressure of the sandblasting device being 0.3 MPa;
[0049] Step STEP103: Provide a raw material of lead-tin bronze alloy powder, which includes 74% copper, 4% tin, and 22% lead.
[0050] Step STEP104: Put the raw material of lead-tin bronze alloy powder into a high-frequency induction melting furnace for vacuum melting, wherein the vacuum degree is set to 6 Pa, the protective gas is argon, the induction power is set to 20 kW, and the induction time is set to 20 min to obtain a molten mixture.
[0051] Step STEP105: After the smelted mixture is completely alloyed, the melt temperature is adjusted to 1200° C., and then the mixture is put into an atomizing device and atomized with argon gas to prepare powder. The vacuum atomization process conditions include selecting high-purity argon gas as a protective gas, a vacuum degree of 5×104 Pa, and an atomization pressure of 3.5 to 3.6 MPa. The lead-tin bronze alloy powder is subjected to particle size screening and powder drying, and then vacuum-packaged to obtain the lead-tin bronze alloy powder;
[0052] Step STEP106: using cold spraying technology to spray lead-tin bronze alloy powder onto the surface of the substrate, with a thickness of 1 to 3 mm and a bonding force of 10 to 200 MPa;
[0053] Step STEP107: Use a laser cladding machine to heat the lead-tin bronze alloy powder to a target temperature of 820°C until the copper layer on the surface of the entire substrate is heated to achieve metallurgical bonding with a bonding force of 200 MPa, a laser power of 3000 W, and a line speed of 600 mm / min.
[0054] Comparative Example 1
[0055] The manufacturing method of the wind power sliding bearing of this embodiment comprises the following steps:
[0056] 1) Prepare a bearing matrix, place the bearing matrix horizontally, and allow the bearing matrix to rotate around the central axis of the bearing matrix.
[0057] 2) Spraying lead-tin bronze powder and laser beam on the surface of the bearing matrix simultaneously, intersecting the tin bronze powder and laser beam before spraying onto the surface of the bearing matrix, so as to form a cladding layer in the cladding area of the bearing matrix. The tin-copper powder is an existing material.
[0058] 3) Move the cladding area along the axial direction of the bearing matrix and repeat step 2) until a cladding layer is formed on the entire surface of the bearing matrix.
[0059] exist Figure 2 and Figure 3 , which are metallographic images of Practical Example 1 and Comparative Example 1 obtained at the same magnification. Figure 2 This is the metallographic diagram of Example 1. Figure 3 It is the metallographic diagram of comparative example 1. Figure 2 In the graph, lead particles are the black part, which is Figure 3 In comparison, it is obviously smaller and evenly distributed without obvious segregation.
[0060] Compared with the prior art, the preparation method of the lead-containing copper alloy sliding bearing for the wind power gearbox provided by the present invention adopts the lead-containing copper alloy, while ensuring the load-bearing capacity, it also takes into account the compliance and anti-bite property. Specifically, due to the presence of lead, the lubricity of the bearing material is improved, which is conducive to improving the compliance and anti-bite property of the bearing material. However, due to the presence of lead, higher requirements are placed on its preparation method, especially using the laser cladding process. Specifically, due to the high temperature of the laser cladding process, if the lead-containing copper alloy powder is directly clad on the substrate, it will not only aggregate but also segregate. In the present preparation method, the lead-containing copper alloy is formed into small metal droplets by an atomization process, and then the lead-containing tin bronze powder is sprayed on the substrate by cold spraying, so that the lead can be evenly covered on the substrate, and finally the lead-containing tin bronze layer is melted by the laser cladding process, which can prevent the lead from segregating at high temperature, thereby causing uneven distribution, so that the compliance and anti-bite property of the obtained bearing material can be guaranteed.
[0061] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modification, equivalent substitution or improvement within the spirit of the present invention is included in the scope of the claims of the present invention.
Claims
1. A method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox, comprising the following steps: STEP 101: Provide a substrate and place the substrate horizontally; STEP102: sandblasting the substrate; STEP 103: Provide a raw material of lead-tin bronze alloy powder, and provide an atomizing device to prepare uniformly distributed spherical lead-tin bronze alloy powder, wherein the raw material of the lead-tin bronze alloy powder is composed of Cu, Sn, and Pb, wherein the percentage of Sn in the raw material of the tin bronze alloy powder is 2-15%, the percentage of Pb is 2-24%, and the rest is copper, and the particle size of the prepared lead-tin bronze alloy powder is 10-150 um; STEP 104: Spraying lead-tin bronze powder onto the substrate by cold spraying; STEP 105: Use laser heating to heat the lead-tin bronze powder to a super solid phase sintering temperature of 750-900°C, so that the lead-tin bronze powder and the matrix are metallurgically bonded, and the bonding force reaches more than 200 MPa to complete the preparation of the lead-containing copper alloy sliding bearing.
2. The method for preparing the lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: The substrate is one of a copper shaft and an alloy shaft.
3. The method for preparing the lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: In step STEP102, during the sand blasting process, the substrate surface is sandblasted to remove oil stains and oxide scale on the substrate surface and to roughen the substrate. The output pressure of the sand blasting equipment is 0.3 MPa.
4. The method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 3, characterized in that: The sand used in the sandblasting process is one of brown corundum, white corundum and garnet sand.
5. The method for preparing the lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: In step STEP 105 , the equipment used for the laser heating method is a laser cladding machine.
6. The method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 5, characterized in that: The laser cladding machine is operated along the axial direction of the substrate. After heating to the end, the substrate is rotated by a certain angle and continues to be heated along the axial direction until the entire substrate is completely heated.
7. The method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: The equipment used for the laser heating is a laser cladding machine, the power of which is between 1000 and 5000 W, and the line speed is between 600 and 1800 mm / min.
8. The method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: The raw materials of the lead-tin bronze alloy powder include 74% copper, 4% tin and 22% lead.
9. The method for preparing a lead-containing copper alloy sliding bearing for a wind power gearbox according to claim 1, characterized in that: In STEP 103, the raw material of lead-tin bronze alloy powder is put into a high-frequency induction melting furnace for vacuum melting, wherein the vacuum degree is set to 6 Pa, the protective gas is argon, the induction power is set to 20 kW, and the induction time is set to 20 min to obtain a molten mixture.
Citation Information
Cited By
Preparation method for preparing high-strength copper-lead alloy through laser-assisted cold spraying