Self-repairing antibacterial hydrogel, preparation method and application thereof

By adding high-molecular-weight proluranol to polyvinyl alcohol and borax hydrogels to form borate ester bonds and hydrogen bonds, the problem of insufficient versatility of hydrogel materials in the biomedical field is solved, and high-molecular-weight prolurgy is achieved The adhesion, self-healing and antibacterial properties of Rulandosaccharide hydrogels are improved, suitable for a variety of surfaces and applications.

CN118546436BActive Publication Date: 2024-11-08JIANGSU OCEAN UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410623963.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-08
Estimated Expiration
2044-05-20

AI Technical Summary

Technical Problem

The existing hydrogel materials lack versatility in the field of biomedical science, especially the difficulty in having good adhesion, antibacteriality and self-repairability at the same time, limiting their use in practical applications.

Method used

A chemical borate ester bond hydrogel formed by polyvinyl alcohol and borax is added with high molecular weight plulandosaccharide, which improves the mechanical properties, self-healing ability and antibacterial properties of the hydrogel through the formation of borate ester bonds and hydrogen bonds.

Benefits of technology

The prepared hydrogel has good adhesion and self-healing properties, can heal itself without external stimulation at room temperature, and has a broad-spectrum antibacterial effect on a variety of bacteria. It is suitable for skin, rubber, glass, metal and other surfaces. Adhesion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546436B_ABST
    Figure CN118546436B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-healing antibacterial hydrogel, a preparation method and an application thereof. The present invention combines a boronate bond and a hydrogen bond to prepare a hydrogel with adhesion, self-healing and antibacterial properties. The hydrogel is based on polyvinyl alcohol (PVA) as a base network and a borax solution as a cross-linking agent, and a boronate bond is formed between the two. Pullulan (Pullulan) containing a large number of hydroxyl groups is added to form hydrogen bonds, which increases the viscosity of the hydrogel and can adhere to the surfaces of objects such as skin, rubber, glass, metal and plastic. Rheological and tensile tests show that the hydrogel after adding pullulan can self-heal within 80s, which is 60s longer than that without pullulan; the tensile strain of the hydrogel is increased by 393%, and the tensile strength is increased by 0.047MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogels, and in particular relates to a self-repairing antibacterial hydrogel, a preparation method and application thereof. Background Art

[0002] Pullulan, also known as pullulan, is a linear polysaccharide composed of maltotriose linked by α-1,4 glycosidic bonds as repeating units. The maltotriose is linked by α-1,6 glycosidic bonds. The structure of the two glycosidic bonds arranged in a regular alternating pattern gives pullulan many excellent physical and chemical properties, such as plasticity, biocompatibility, high bioadhesion, biodegradability, and non-toxicity. It is accepted by the FDA and the European Union as a safe biopolymer and is widely used in food packaging, drug excipients for drug delivery systems, wound healing, tissue engineering and other fields.

[0003] With the rapid development of polymer science and life science, hydrogel materials have received great attention. In particular, due to the unique similarity between hydrogel materials and biological tissues, as well as their versatility and flexibility in tailoring properties, they have become a research hotspot in the fields of biomedicine and tissue engineering. In the field of biomedical engineering, the development of hydrogel materials usually requires properties such as hemostasis, antibacterial, self-repair, and tissue adhesion. Usually, hydrogel materials have only one property and cannot meet the application of actual application scenarios, so it is necessary to research and develop hydrogel materials with multiple properties.

[0004] Self-healing hydrogels are a type of hydrogel that can restore its structure and function autonomously after damage, either autonomously or by relying on external stimuli. There are many self-healing mechanisms of hydrogels, which can be divided into two categories according to the formation of their internal networks: dynamic chemical covalent cross-linking and physical non-self-healing. The main common dynamic covalent bonds are imine bonds, Diels-Alder (DA) reactions, boronate bonds, and disulfide bonds, while the main common physical non-covalent interactions are hydrogen bonds, hydrophobic interactions, and host-guest interactions. The chemical boronate bonds formed by cross-linking polyvinyl alcohol (PVA) and borax are reversible and are often used to synthesize fast self-healing hydrogels, but this type of hydrogel PVA / borax hydrogel does not have good mechanical properties and fast self-healing properties, which limits its practical application range. With the development of public health and biomedical technology, the number of drug-resistant pathogens is increasing, and hydrogels with antibacterial properties have gradually attracted the interest of researchers. Although the application of antibacterial hydrogels in the biomedical field has been studied, their application in actual bioengineering still faces many challenges. Single-functional hydrogels are no longer able to meet usage requirements; therefore, research on hydrogels with adhesion, antibacterial properties and self-healing properties has very important scientific significance and broad application prospects.

[0005] The molecular weight of the pullulan currently available on the market is generally around 10 5 The mechanical strength is insufficient, which greatly limits the application of pullulan. Patent announcement number CN115353979B discloses a strain of Pullulan polysaccharide YAT007 that produces high molecular weight pullulan polysaccharide and its application. The pullulan polysaccharide produced by fermentation by the strain has a molecular weight of 10 7 High molecular weight pullulan hydrogel can effectively solve the technical problems of poor mechanical properties and slow self-healing speed of polyvinyl alcohol (PVA)-borax. Summary of the invention

[0006] The present invention is based on a chemical borate ester bond hydrogel formed by polyvinyl alcohol and borax, and high molecular weight pullulan is added. The high molecular weight pullulan contains a large number of hydroxyl groups, which can increase the mechanical properties and self-healing ability of the hydrogel. The adhesion performance, self-healing property and antibacterial property of the pullulan / borax / polyvinyl alcohol hydrogel are further characterized and tested to obtain a self-healing antibacterial hydrogel.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A self-repairing antibacterial hydrogel, characterized in that the hydrogel is formed by cross-linking reaction of polyvinyl alcohol, pullulan and borax aqueous solution.

[0009] Polyvinyl alcohol is 0.2 g, pullulan is 0.5-1 g, and 20% borax aqueous solution.

[0010] A method for preparing the self-healing antibacterial hydrogel according to claim 1, the method being as follows: adding polyvinyl alcohol (PVA) to distilled water, stirring in a 90°C water bath to completely dissolve; adding pullulan; stirring the sample mixed solution evenly, adding 20% ​​borax aqueous solution at 10% of the total volume of the mixed solution, the cross-linking reaction is completed rapidly, the solution gradually becomes gel-like, and after being taken out in time, it is placed in a mold and left to stand to form a stable hydrogel.

[0011] The invention discloses an application of a self-healing antibacterial hydrogel. The hydrogel is used in antibacterial applications, specifically having antibacterial effects on two Gram-positive bacteria, Staphylococcus aureus, Listeria monocytogenes, and seven Gram-negative bacteria, Escherichia coli, Aeromonas hydrophila, Salmonella typhi, Edwardsiella tarda, Vibrio anguillarum, Aeromonas enterica, and Shewanella.

[0012] The following beneficial effects can be obtained through the above technical solution:

[0013] The present invention solves and provides a pullulan hydrogel with good adhesion, self-healing properties and antibacterial properties. The results of infrared spectroscopy FT-IR show that the tetraborate ions in borax and the hydroxyl groups in the polyvinyl alcohol chain are easy to form borate ester bonds, that is, a chemical cross-linked network. Pullulan also has a certain number of hydroxyl groups, which are cross-linked with the polyvinyl alcohol network to form hydrogen bonds, which are physical cross-linked networks. The complexation of tetraborate ions with the hydroxyl groups of polyvinyl alcohol is reversible, and self-healing tests show that the hydrogel has good self-repairing properties. The structure containing phenol in the borate ester bond makes the hydrogel antibacterial, and the antibacterial test shows that the hydrogel has a broad spectrum. The network between pullulan and polyvinyl alcohol will provide a stable structure to withstand stress, thereby improving the adhesion and stability of the hydrogel.

[0014] The hydrogel of the present invention can adhere to the surface of objects such as skin, rubber, glass, metal and plastic. The rheological and adhesion tests show that the hydrogel has good adhesion. Due to the uniqueness of the borate bond, the hydrogel can heal itself at room temperature without additional stimulation. The hydrogel prepared by the present invention has a broad-spectrum antibacterial effect, and has a certain antibacterial effect on two Gram-positive bacteria Staphylococcus aureus and Listeria monocytogenes and seven Gram-negative bacteria Escherichia coli, Vibrio anguillarum, Edwardsiella tarda, Aeromonas enterica, Shewanella, Salmonella typhi, and Aeromonas hydrophila.

[0015] The invention is based on the chemical borate ester bond hydrogel formed by polyvinyl alcohol and borax, and adds black pigment-producing short-stalked mold Aureobasidium melanogenum The high molecular weight pullulan fermented by YAT007 (deposit number CGMCC 40201) contains a large number of hydroxyl groups, which will increase the mechanical properties and self-healing ability of the hydrogel, and further enhance the adhesion, self-healing and antibacterial properties of the hydrogel. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 (A) Infrared spectroscopic analysis of borax, polyvinyl alcohol and pullulan;

[0017] (B) FT-IR analysis of hydrogels (P-1) 2% PVA-20% Borax (P-2) 5% Pullulan-2% PVA-20% Borax (P-3) 7% Pullulan-2% PVA-20% Borax (P-4) 10% Pullulan-2% PVA-20% Borax;

[0018] (C) C 1s spectrum of hydrogel;

[0019] (D) Hydrogel O 1s spectrum;

[0020] (E) 1s spectrum of hydrogel B.

[0021] Figure 2 (A) 5 μm SEM image of the hydrogel; (B) 10 μm SEM image of the hydrogel.

[0022] Figure 3 This is the viscosity change diagram of hydrogel when the shear rate is 0.01~100 1 / s (P-1) 2% PVA-20% Borax; (P-2) 5% Pullulan-2% PVA-20% Borax; (P-3) 7% Pullulan-2% PVA-20% Borax; (P-4) 10% Pullulan-2% PVA-20% Borax.

[0023] Figure 4 (AC) Hydrogel self-healing behavior.

[0024] (D) P-1 strain amplitude scan.

[0025] (E) P-1 alternating step strain scan.

[0026] (F) P-2 strain amplitude scan.

[0027] (G) P-2 alternating step strain scan.

[0028] Figure 5 (A) The hydrogel adheres to the finger and can be bent from 0° to 90° and finally restored to 0°; (B), (C) The adhesion performance of the hydrogel to the surfaces of different materials; (D) Schematic diagram of the hydrogel's bearing capacity.

[0029] Figure 6 (A) Staphylococcus aureus (P-1) 2% PVA-20% Borax, (P-2) 5% Pullulan-2% PVA-20% Borax, (P-3) 7% Pullulan-2% PVA-20% Borax, (P-4) 10% Pullulan-2% PVA-20% Borax;

[0030] (B) Listeria monocytogenes;

[0031] (C) Escherichia coli;

[0032] (D) Aeromonas hydrophila;

[0033] (E) Salmonella typhi;

[0034] (F) Edwardsiella tarda;

[0035] (G) Vibrio anguillarum;

[0036] (H) Aeromonas enterica;

[0037] (I) Shewanella.

[0038] Figure 7 : Hydrogel tensile strain-tensile strength diagram. DETAILED DESCRIPTION

[0039] The following is combined with Figure 1-7 The present invention is further described with examples:

[0040] The pullulan is produced by a high-molecular-weight pullulan-producing strain, which is classified and named as Melaninogenic Atractylodis Macrocephala ( Aureobasidium melanogenum )YAT007, on May 23, 2022, was deposited in the General Microbiology Center of China Microorganism Culture Collection Administration, and the deposit number is CGMCC NO:40201.

[0041] The method for producing pullulan by the strain of Acidis melanoderma pullulans YAT007 comprises the following steps:

[0042] Activation of strains: Transfer the melanin-producing Aureobasidium brevifolium YAT007 strain stored on a 4 ℃ slant to PDA medium and culture at 28 ± 2 ℃ for 4-6 days;

[0043] Seed culture: Pick a single colony of YAT007 strain and inoculate it into 30 mL seed culture medium at 28 °C and 180 rpm for 24 h.

[0044] Fermentation culture: transfer the seed solution to 50 mL of fermentation medium at a 10% (v / v) inoculation rate and culture at 28 °C, 180 rpm for 120 h.

[0045] Extraction and purification of extracellular polysaccharides: After fermentation, take 30 mL of fermentation liquid to a 50 mL centrifuge tube, centrifuge at 12000 × g for 10 min, boil the supernatant at 100 ° C for 15 min, centrifuge at 12000 × g for 10 min, cool to room temperature, take 10 mL of supernatant to a new 50 mL centrifuge tube, add 20 mL of pre-cooled anhydrous ethanol, mix well, and let stand at 4 ° C overnight for precipitation. Centrifuge at 9000 × g, 4 ° C for 5 min, discard the supernatant, and bake at 80 ° C to constant weight. After the crude extracellular polysaccharide is dissolved in sterile deionized water, it is repeatedly precipitated and extracted with ethanol for purification to finally obtain pullulan.

[0046] 0.2 g of polyvinyl alcohol (PVA) was added to 10 mL of distilled water and stirred in a 90 °C water bath until completely dissolved. No pullulan was added, marked as P-1; 0.5 g of pullulan was added, marked as P-2; 0.7 g of pullulan was added, marked as P-3; 1 g of pullulan was added, marked as P-4. The sample mixed solution was stirred evenly, and 20% borax aqueous solution was added according to 10% of the total volume of the mixed solution. The cross-linking reaction was completed quickly, and the solution gradually became gel-like. After being taken out in time, it was placed in a mold and left to stand for 5 minutes to form a stable hydrogel.

[0047] According to the preparation method of (2), P-1, P-2, P-3, and P-4 hydrogels were prepared respectively and dried at 40 °C to constant weight. Potassium bromide was dried at 100 °C to constant weight. Appropriate amounts of polyvinyl alcohol, pullulan, borax, P-1, P-2, P-3, and P-4 sample powders were weighed in a ratio of 1:50-1:100 and ground thoroughly with potassium bromide in an agate mortar, and then the powder samples were pressed into tablets using a tablet press. The test conditions were: scanning range 4000 cm −1 ~400 cm −1 , scanning resolution is 4 cm −1 All samples were tested in triplicate.

[0048] The surface elemental composition and binding valence of the samples were determined using XPS with an excitation source of (Al K Alpha) at an energy of approximately 29.35 eV.

[0049] The hydrogel was prepared according to the preparation method (2) and pre-frozen at -80 °C, and freeze-dried in a freeze dryer for 24 h. The freeze-dried hydrogel was coated with a metal film and finally observed and photographed using a scanning electron microscope.

[0050] P-1, P-2, P-3, and P-4 hydrogels were prepared according to the preparation method of (2). The rheological properties of the hydrogels were tested by MCR 102 rheometer. The test conditions were as follows: 1. Select the constant shear mode with a shear rate of 0.01 ~ 100 1 / s to observe the viscosity changes of the hydrogels at different shear rates.

[0051] In a mixed solution of pullulan / polyvinyl alcohol, Congo red (red) and methylene blue (blue) were loaded into the mixed solution, and then poured into a mold after adding borax solution, so that the hydrogel appeared red and blue. The red and blue hydrogels of the same shape were cut into two halves of the same size. At room temperature, the cut surfaces of the hydrogels of different colors were placed in contact with each other without any external intervention, and the self-healing phenomenon of the hydrogel was observed. The self-healing hydrogel and the stretching condition were photographed and recorded.

[0052] Test the adhesion of hydrogel to different materials including skin, rubber, glass, metal, cotton, linen, leaves, paper, film, polytetrafluoroethylene, and polypropylene.

[0053] Bacterial culture

[0054] Two Gram-positive bacteria, Staphylococcus aureus and Listeria monocytogenes, and seven Gram-negative bacteria, Escherichia coli, Vibrio anguillarum, Edwardsiella tarda, Aeromonas enterica, Shewanella spp., Salmonella typhi, and Aeromonas hydrophila, were selected as indicator bacteria to test the antibacterial properties of the hydrogel.

[0055] Streak the indicator bacteria on the LB plate medium and culture at 37 ℃ for 1 day. Take a small amount of bacteria from the activated LB medium with a sterile inoculation loop and inoculate it into 5mL LB liquid medium. Culture it at 37 ℃ and 180 rpm for 8 to 16 hours. Use a UV spectrophotometer to measure the absorbance value (OD600) of the bacterial solution at 600 nm to determine the concentration of the bacterial solution to be 0.8~1 for later use.

[0056] Antibacterial experiment

[0057] The experimental plates were prepared by pouring the pre-added bacterial solution into the plate: 500uL of indicator bacterial solution was injected into 50mL of 1% agar LB plate medium that had been cooled to about 40°C, mixed evenly, and poured into a plate with an Oxford cup of 8 mm in diameter (about 20mL / plate). After it was allowed to stand horizontally until solidified, the Oxford cup was removed with tweezers and set aside.

[0058] Weigh 0.2 g of the P-1, P-2, P-3, and P-4 hydrogels prepared according to the preparation method (2) and place them in a clean bench for UV sterilization for 2 hours. Then, place them in the holes in the Oxford cup and place the plates upright in a 37 °C incubator for 24 hours. Take photos and measure the diameter of the inhibition zone.

[0059] According to the preparation method of (2), P-1 and P-2 hydrogels were prepared respectively, and the tensile properties of the hydrogels were tested using a universal testing machine. The hydrogel samples were placed in a rectangular mold with a length of 30 mm, a width of 10 mm, and a thickness of 4 mm. The length of the test hydrogel (i.e., the initial length of the hydrogel) was 20 mm, and the tensile speed was 80 mm / min.

[0060] The hydrogel was observed by infrared spectroscopy FT-IR and X-ray photoelectron spectroscopy XPS. The results of infrared spectroscopy FT-IR ( Figure 1 As shown in A and B, the 1420 cm −1 The characteristic peak at 3100~3700 cm is attributed to the asymmetric stretching vibration of BOC bond, which indicates the existence of borate ester bonds in the hydrogel. -1In the spectrum of PVA, the 1150 cm -1 The absorption peak at 3428 cm in P-1 hydrogel is related to the stretching mode of CO in PVA. -1 The characteristic peak of -OH in P-2 hydrogel moved to 3418 cm -1 , which means that there are hydrogen bonding interactions between polyvinyl alcohol, borax and pullulan. Similarly, more signal shifts can be observed. After the addition of pullulan to P-1 hydrogel, a signal shift at 1020 cm −1 The characteristic absorption band at is the stretching absorption peak of the α-1,6-D glucoside bond of pullulan. X-ray photoelectron spectroscopy XPS results ( Figure 1 C, D, and E) further confirmed the successful preparation of pullulan / polyvinyl alcohol / borax hydrogel. Figure 1 The CO and OH absorption peaks in C and D come from polyvinyl alcohol and pullulan. After adding borax, CB and BO absorption peaks appear. The results BO and BC in Figure E indicate that the hydrogel contains borate bonds.

[0061] like Figure 2 The scanning electron microscopy results of P-2 hydrogel showed that the cross-section of the freeze-dried hydrogel had an obvious regular network structure, showing an interconnected porous structure. Such a highly porous hydrogel has good water absorption properties and can provide space for cell attachment, growth, migration, secretion, infiltration, differentiation and vascularization.

[0062] like Figure 3 The shear rate-viscosity rheology of the hydrogels shows that the viscosity of the hydrogels increases with the increase of the polysaccharide concentration, and the viscosity of the four hydrogels decreases with the increase of the shear rate, indicating that they have shear thinning properties. The shear thinning ability of the pullulan-polyvinyl alcohol-borax hydrogel is proved, which has potential application prospects for injectable hydrogels.

[0063] like Figure 4 The self-healing test results of AC hydrogel (represented by P-2 hydrogel) show that two hydrogels loaded with different colors (methylene blue and Congo red) were cut into two pieces respectively, and the two gel pieces of different colors were brought into contact with each other. Once they were in contact, the self-healing of the gel occurred immediately, and after 1 minute of close combination, it became a whole gel piece. The self-healed hydrogel can be stretched without damage. Figure 4The results of the strain amplitude scan of hydrogel P-1 show that the intersection of the storage modulus (G') and the loss modulus (G'') of P-1 is 893%, indicating that the network structure of P-1 is destroyed at this intersection. Therefore, 1% - 900% was selected as the alternating strain to further determine the self-healing behavior of P-1. Figure 4 It can be seen from Figure E that when the strain of P-1 is 1%, G' is 82.87 Pa, G'' is 38.52 Pa, G' is greater than G'', and P-1 is in a gel state. When the strain increases to 900%, G' drops sharply to only 2.33 Pa, and G'' (4.69 Pa) is greater than G', indicating that the network structure of P-1 is destroyed at this time. When the strain returns to 1%, the G' of P-1 immediately recovers to 80.37 Pa, and G'' is 38.567 Pa, indicating that the network structure of P-1 is restored to a complete state at this time, which can be completed within 140 s. Figure 4 The results of strain amplitude scanning of F hydrogel P-2 show that the intersection of storage modulus (G') and loss modulus (G'') of P-2 is 296%, indicating that the network structure of P-2 hydrogel is destroyed at this intersection. Therefore, 1% - 300% was selected as the alternating strain to further determine the self-healing behavior of P-2. Figure 4 It can be seen from G that when the strain of P-2 is 1%, G' is 1329.7 Pa, G'' is 692.76 Pa, G' is greater than G'', and P-2 is in a gelation state. When the strain increases to 300%, G' decreases sharply to only 251.18 Pa, and G'' (336.04 Pa) is greater than G', indicating that the network structure of P-2 is destroyed at this time. When the strain is restored to 1%, the G' of P-1 is immediately restored to 964.13 Pa, and G'' is 565.33 Pa, indicating that the network structure of P-2 is restored to a complete state at this time, and the recovery is rapid, which can be completed within 80 s. According to the above results, the P-1 hydrogel can complete the self-healing process within 140 s, and the P-2 hydrogel after adding pullulan can complete the self-healing process within 80 s, and the self-healing time is increased by 60 s. Its self-healing process does not require the intervention of external factors, laying the foundation for its application in medicine, materials and other fields.

[0064] like Figure 5 As shown in the results of the hydrogel adhesion test, when the hydrogel (represented by P-2 hydrogel) is adhered to the finger joints, the joints are bent 45°, 90°, and then restored to 0°, the hydrogel can still adhere well to the skin, and the hydrogel maintains its shape intact and does not fall off. Figure 5 As shown in B and C, the hydrogel has excellent interfacial adhesion behavior on various substrate interfaces (including rubber, glass, metal, cotton and linen, etc.). Figure 5As shown in Figure D, the glass slide and polypropylene material can be tightly adhered through the hydrogel to support the weight of 10 g and 50 g; the two glass slides can be tightly adhered through the hydrogel to support the weight of 50 g and 100 g. The above results show that the hydrogel has good adhesion.

[0065] The antibacterial properties of P-1, P-2, P-3 and P-4 hydrogels against Staphylococcus aureus, Listeria monocytogenes, Escherichia coli, Aeromonas hydrophila, Salmonella typhi, Edwardsiella tarda, Vibrio anguillarum, Aeromonas enterica and Shewanella Figure 6 As shown, all of them showed different degrees of antibacterial activity, among which the antibacterial ability against Staphylococcus aureus, Vibrio anguillarum and Shewanella was relatively good. The quantitative results of the inhibition ring size are shown in Table 1. The inhibition results show that the hydrogel has a broad spectrum, among which the inhibition ring sizes of P-1, P-2, P-3, and P-4 hydrogels against Vibrio anguillarum are 19.4 ± 0.06 mm, 17.7 ± mm, 17.63 ± mm, and 17.5 ± mm, respectively.

[0066] Table 1 Antibacterial diameters (mm) of P-1, P-2, P-3, and P-4 hydrogels against indicator bacteria.

[0067] Indicator bacteria P-1 P-2 P-3 P-4 Staphylococcus aureus <![CDATA[12.2±0.06 c ]]> <![CDATA[13.2±0.03 b ]]> <![CDATA[13.2±0.03 b ]]> <![CDATA[14.2±0.06 c ]]> Listeria monocytogenes <![CDATA[10.2±0.04 d ]]> <![CDATA[10.4±0.06 c ]]> <![CDATA[11.39±0.12 b ]]> <![CDATA[14.5±0.07 a ]]> Escherichia coli <![CDATA[12.3±0.06 b ]]> <![CDATA[12.4±0.03 a ]]> <![CDATA[12.4±0.05 a ]]> <![CDATA[12.4±0.00 a ]]> Aeromonas hydrophila <![CDATA[14.1±0.06 a ]]> <![CDATA[13.7±0.07 b ]]> <![CDATA[12.6±0.18 c ]]> <![CDATA[12.5±0.09 c ]]> Salmonella typhi <![CDATA[10.8±0.05 a ]]> <![CDATA[11.4±0.07 b ]]> <![CDATA[12.4±0.06 a ]]> <![CDATA[12.4±0.06 a ]]> Edwardsiella tarda <![CDATA[13.3±0.08 a ]]> <![CDATA[13.4±0.04 a ]]> <![CDATA[13.4±0.06 a ]]> <![CDATA[13.3±0.06 a ]]> Vibrio anguillarum <![CDATA[19.4±0.06 a ]]> <![CDATA[17.7±0.09 b ]]> <![CDATA[17.63±0.12 bc ]]> <![CDATA[17.5±0.04 a ]]> Aeromonas enterica <![CDATA[11.7±0.07 c ]]> <![CDATA[12.5±0.06 b ]]> <![CDATA[13.5±0.05 a ]]> <![CDATA[13.4+0.07 a ]]> Shewanella <![CDATA[13.5±0.05 b ]]> <![CDATA[13.5±0.05 b ]]> <![CDATA[15.6±0.03 a ]]> <![CDATA[15.6±0.03 a ]]>

[0068] like Figure 7 The results of the hydrogel tensile test showed that the tensile strains of P-1 and P-2 were 380% and 773%, respectively. The tensile strengths of P-1 and P-2 were 0.007 MPa and 0.054 MPa. The results showed that the tensile strength and ductility of the hydrogel were improved after the addition of pullulan, with the tensile strain increased by 393% and the tensile strength increased by 0.047 MPa.

[0069] In summary, the present invention combines the method of borate ester bond and hydrogen bond to prepare a hydrogel with adhesion, self-healing and antibacterial properties. The hydrogel is based on polyvinyl alcohol (PVA) as the base network and borax solution as the cross-linking agent, and borate ester bonds are formed between the two. Pullulan (Pullulan) containing a large number of hydroxyl groups is added to form hydrogen bonds, which increases the viscosity of the hydrogel and can adhere to the surfaces of objects such as skin, rubber, glass, metal and plastic. Rheological and adhesion tests show that the hydrogel has good adhesion. Due to the uniqueness of the borate ester bond, the hydrogel can heal itself at room temperature without additional stimulation. The hydrogel prepared by the present invention has a broad spectrum of antibacterial properties, and has a certain antibacterial effect on two Gram-positive bacteria Staphylococcus aureus, Listeria monocytogenes and seven Gram-negative bacteria Escherichia coli, Aeromonas hydrophila, Salmonella typhi, Edwardsiella tarda, Vibrio anguillarum, Aeromonas enterica, and Shewanella. The multifunctional hydrogel developed by the present invention provides more ideas and references for the application of pullulan in practice.

[0070] The above are all preferred embodiments of the present invention. For ordinary technicians in this technical field, without departing from the principle of the present invention, various equivalent modifications to the present invention belong to the protection scope of the claims attached to this application.

[0071] In summary, the present invention combines the method of borate ester bond and hydrogen bond to prepare a hydrogel with adhesion, self-healing and antibacterial properties. The hydrogel is based on polyvinyl alcohol (PVA) as the base network, borax solution as the cross-linking agent, and borate ester bonds are formed between the two. Pullulan (Pullulan) containing a large number of hydroxyl groups is added to form hydrogen bonds, which increases the viscosity of the hydrogel and can adhere to the surfaces of objects such as skin, rubber, glass, metal and plastic. Rheological and adhesion tests show that the hydrogel has good adhesion. Due to the uniqueness of the borate ester bond, the hydrogel can heal itself at room temperature without additional stimulation. The hydrogel prepared by the present invention has a broad spectrum of antibacterial properties, and has a certain antibacterial effect on 2 Gram-positive bacteria Staphylococcus aureus, Listeria monocytogenes and 7 Gram-negative bacteria Escherichia coli, Aeromonas hydrophila, Salmonella typhi, Edwardsiella tarda, Vibrio anguillarum, Aeromonas intestinalis, and Shewanella. The multifunctional hydrogel developed by the present invention provides more ideas and references for the application of pullulan in practice.

[0072] The above are all preferred embodiments of the present invention. For ordinary technicians in this technical field, without departing from the principle of the present invention, various equivalent modifications to the present invention belong to the protection scope of the claims attached to this application.

Claims

1. A self-repairing antibacterial hydrogel, characterized in that: The hydrogel is formed by the cross-linking reaction of polyvinyl alcohol, pullulan and borax aqueous solution; wherein, pullulan is produced by fermentation of a high-molecular-weight pullulan high-yield strain, and the classification and naming of the high-yield strain is Aureobasidium melanogenum YAT007, which was deposited in the General Microbiology Center of the China Microbiological Culture Collection Administration on May 23, 2022, and the deposit number is CGMCC NO:40201.

2. The self-healing antibacterial hydrogel according to claim 1, characterized in that: Polyvinyl alcohol is 0.2 g, pullulan is 0.5-1 g, and 20% borax aqueous solution.

3. A method for preparing the self-healing antibacterial hydrogel according to claim 1, characterized in that: The method is as follows: polyvinyl alcohol (PVA) is added into distilled water, and stirred in a water bath at 90°C to completely dissolve; high molecular weight pullulan from biological fermentation is added; the sample mixed solution is stirred evenly, and a 20% borax aqueous solution is added according to 10% of the total volume of the mixed solution, the cross-linking reaction is completed rapidly, and the solution gradually becomes gel-like. After being taken out in time, it is placed in a mold and left to stand, so that a stable hydrogel can be formed.

4. The use of the self-repairing antibacterial hydrogel according to claim 1, characterized in that: The invention is used for preparing an antibacterial product, which has an antibacterial effect on two gram-positive bacteria, Staphylococcus aureus and Listeria monocytogenes, and seven gram-negative bacteria, Escherichia coli, Aeromonas hydrophila, Salmonella typhi, Edwardsiella tarda, Vibrio anguillarum, Aeromonas enterica, and Shewanella.

Citation Information

Patent Citations

  • A short-stalked fungus strain YAT007 producing high molecular weight pullulan and its application

    CN115353979B

  • Ecological environment-friendly dust inhibitor

    CN103184034A

  • High-extension, high-adhesion and high-self-healing double network hydrogel and preparation method and application thereof

    CN110240712A

  • Hydrogel composition, living tissue model, and method for producing living tissue model

    CN111149144A

  • Ultrafast self-healing polysaccharide-based hydrogel strain sensor and manufacturing method thereof