A kind of environmentally friendly styrene-butadiene latex with enhanced viscosity and preparation method thereof

CN118562207BActive Publication Date: 2024-11-05潍坊蓝励新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044806.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-05
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing styrene butadiene latex has low viscosity in asphalt modification, which cannot meet the needs of improving the bonding force, wear resistance and anti-aging properties of asphalt.

Method used

The viscosity-enhancing and environmentally friendly styrene butadiene latex is prepared through low-temperature emulsion polymerization process. A specific proportion of emulsifiers, carboxylic acid monomers, initiators, molecular weight regulators and defoamers are used to control the polymerization reaction conditions and the addition sequence, and improve the butadiene and The conversion rate of styrene and the molecular weight distribution of the polymer are finally added to adjust the viscosity.

Benefits of technology

It significantly improves the viscosity of styrene butadiene latex, with uniform average particle size, ≥483 mpas/25℃, and has high stability. It is suitable for road paving and building materials in cold areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of styrene butadiene latex, and in particular to a tackified environmentally friendly styrene butadiene latex and a preparation method thereof, comprising the following steps: adding deionized water, an emulsifier, a carboxylic acid monomer, a molecular weight regulator, and a defoamer into a reactor to obtain an aqueous emulsion; introducing nitrogen into the polymerization reactor for replacement three times and evacuating the reactor, distributing the aqueous emulsion in the reactor to the polymerization reactor, cooling the reactor, adding butadiene and styrene for polymerization reaction; adding a molecular weight regulator and an electrolyte, and continuously stirring; adding a terminator to terminate the polymerization reaction; after the reaction is completed, adding sodium alginate and polyacrylamide, stirring, and obtaining styrene butadiene latex. The styrene butadiene latex produced by the method has a uniform particle size distribution, an average particle size distribution of 281.5nm, a viscosity of ≥483mpas / 25°C, and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of styrene butadiene latex, in particular to a tackifying environmentally friendly styrene butadiene latex and a preparation method thereof. Background Art

[0002] Styrene butadiene latex, full name styrene butadiene rubber emulsion, is a white milky liquid made from butadiene and styrene through emulsion polymerization. This latex is one of the important products in the rubber industry, with unique physical and chemical properties, making it widely used in many fields.

[0003] The viscosity characteristic of styrene butadiene latex is one of its important physical properties, which has a direct impact on its application performance. In highway engineering, high-viscosity, large-particle-size styrene butadiene latex is often used for asphalt modification. By mixing it with asphalt, the adhesion, wear resistance and anti-aging properties of asphalt can be significantly improved, thereby extending the service life of the road. However, at the same solid content, the larger the particle size, the lower the viscosity value. This is because the interaction between large particles is weak, and lower shear force is required for flow, which manifests as lower viscosity and cannot meet the modification requirements.

[0004] Therefore, it is of great significance to study a high-viscosity, large-particle-size styrene-butadiene latex to improve the adhesion, wear resistance and anti-aging properties of asphalt. Summary of the invention

[0005] In view of the defects mentioned in the background technology, the present invention provides a method for preparing a tackified environmentally friendly styrene-butadiene latex, which is specifically achieved by the following technical scheme:

[0006] A method for preparing a tackified environmentally friendly styrene-butadiene latex comprises the following steps:

[0007] S1. Add 280-320 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C;

[0008] S2, adding 5 to 15 parts of emulsifier, 2.5 to 6 parts of carboxylic acid monomer, 1.5 to 2 parts of initiator, 1 to 2 parts of molecular weight regulator, and 0.6 to 1.8 parts of defoamer into deionized water, maintaining the above temperature and stirring and dispersing for 0.5 to 1 hour, stopping heating, cooling to room temperature, and obtaining an aqueous emulsion;

[0009] S3, prepare at least two polymerization kettles to form a production line, introduce nitrogen into the kettle for replacement three times and evacuate, distribute the aqueous emulsion in the reactor to each polymerization kettle through a metering pump, turn on the agitator, and introduce a refrigerant into the jacket of the polymerization kettle to cool it down. When the temperature in the kettle drops to 5°C, add 30-35wt% of butadiene and 10-15wt% of styrene accounting for the added aqueous emulsion, maintain the temperature in the kettle, and carry out polymerization reaction;

[0010] S4, taking samples, determining the styrene conversion rate by liquid chromatography, when the conversion rate reaches 35-40%, adding 0.3-0.5wt% of the molecular weight regulator and 0.5-1.5wt% of the electrolyte to the added aqueous emulsion, and continuing stirring;

[0011] S5. When the conversion rate reaches 85-90%, adding a terminator accounting for 0.2-0.5 wt % of the added aqueous emulsion to terminate the polymerization reaction;

[0012] S6. After the reaction is completed, stop cooling, add 0.5-1.5wt% of sodium alginate and 0.5-1wt% of polyacrylamide, respectively, and stir for 0.5-1h to obtain styrene-butadiene latex.

[0013] Preferably, in step S6, the styrene-butadiene latex discharged from all polymerization kettles is collected into a buffer tank, the styrene-butadiene latex coming out of the buffer tank is passed through a flash evaporator to recover the incompletely reacted butadiene, the styrene-butadiene latex from which butadiene is removed enters a stripping tower to remove the incompletely reacted styrene, the styrene-butadiene latex from which styrene is removed flows out from the bottom of the stripping tower and is then stored in a finished product tank.

[0014] Preferably, the emulsifier is composed of palm sorbitan and sodium rosinate mixed in proportion, and the weight ratio of sodium rosinate to palm sorbitan is 3:1.

[0015] Preferably, the carboxylic acid monomer is composed of methacrylic acid and acrylic acid in a certain proportion, and the acrylic acid accounts for 45-55% of the total mass of the carboxylic acid monomer.

[0016] Preferably, the initiator is composed of diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, and the ferrous sulfate accounts for 20-25% of the total mass of the initiator.

[0017] Preferably, the molecular weight regulator is tert-dodecyl mercaptan.

[0018] Preferably, the defoaming agent is a polyether-modified silicone oil emulsion.

[0019] Preferably, the electrolyte is potassium chloride.

[0020] Preferably, the terminator is sodium dimethyldithiocarbamate.

[0021] The invention also discloses a tackified environmentally friendly styrene butadiene latex. The viscosity of the styrene butadiene latex obtained by the preparation method is significantly enhanced, and the viscosity is ≥483 mpas / 25°C.

[0022] After adopting the above technical solution, the beneficial effects of the present invention are:

[0023] The styrene butadiene latex produced by the technology of the present invention is formed by low-temperature emulsion polymerization, and thus has excellent low-temperature elongation. This property enables the low-temperature styrene butadiene latex to perform well in application scenarios requiring good low-temperature performance, such as road paving and building materials in cold regions; the produced styrene butadiene latex has a uniform particle size distribution, an average particle size distribution of 281.5 nm, a viscosity of ≥483 mpas / 25°C, and high stability. DETAILED DESCRIPTION

[0024] The features and exemplary embodiments of various aspects of the present invention will be described in detail below. In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only configured to explain the present invention and are not configured to limit the present invention. For those skilled in the art, the present invention can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present invention by illustrating examples of the present invention.

[0025] The directional words appearing in the following description are all directions shown in the figures, and do not limit the specific structure of the present invention. In the description of the present invention, it should also be noted that, unless otherwise clearly specified and limited, the terms "installation" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.

[0026] The styrene-butadiene latex produced by the technology of the present invention is formed by low-temperature emulsion polymerization and thus has excellent low-temperature elongation. This property enables the low-temperature styrene-butadiene latex to perform well in application scenarios requiring good low-temperature performance, such as road paving and building materials in cold regions.

[0027] Example 1

[0028] Preparation of LL-300A styrene-butadiene latex.

[0029] S1. Prepare deionized water

[0030] First, according to the mass fraction, add 280 parts of deionized water into the reactor as the reaction medium to ensure that there is no interference from impurity ions in the reaction system to improve the purity and stability of the product. Turn on the stirring device and heat the reaction system to 38-45°C to allow the chemical substances added later to be better dissolved or dispersed in the deionized water.

[0031] S2. Prepare aqueous emulsion

[0032] Add 5 parts of emulsifier, 2.5 parts of carboxylic acid monomer, 1.5 parts of initiator, 1 part of molecular weight regulator and 0.6 parts of defoamer to the heated and stirred deionized water, and stir the mixture for 0.5 to 1 hour while maintaining the above temperature (38-45°C) to fully dissolve or disperse all the added chemicals in the water. After stirring, stop heating the reactor and let the reaction system cool naturally to room temperature (to prepare for the subsequent polymerization reaction, to ensure that the temperature of the reaction system is in a suitable temperature range when adding monomers for polymerization), to form a uniform aqueous emulsion.

[0033] Emulsifiers play a vital role in emulsion polymerization. They can reduce the surface tension between monomers (butadiene, styrene) and deionized water, allowing the monomers to be stably dispersed in deionized water to form an emulsion. This dispersed state is conducive to the contact and collision between monomer molecules, thereby increasing the chance of polymerization reaction.

[0034] The emulsifier used is composed of palm sorbitan and sodium rosinate in a certain proportion. Palm sorbitan is a non-ionic emulsifier with good emulsification, dispersion and stability. Sodium rosinate is an anionic emulsifier with strong emulsification ability and good water solubility, and can form a stable emulsion in deionized water.

[0035] Palm sorbitan and sodium rosinate can produce a synergistic effect when compounded. This synergistic effect is reflected in their ability to work together in the emulsion system, with a comprehensive effect that is better than a single emulsifier, improving the stability and emulsification efficiency of the emulsion. The weight ratio of sodium rosinate to palm sorbitan is 3:1. After compounding, the HLB value (hydrophile-lipophile balance) of the emulsifier can be accurately controlled to meet the current emulsification needs, making the emulsifier have the best emulsification effect and stability.

[0036] In the process of preparing styrene-butadiene latex, methacrylic acid and acrylic acid are added as carboxylic acid monomers, with acrylic acid accounting for 45% of the total mass of the carboxylic acid monomers, to improve the performance of the latex and form stronger chemical bonds, thereby increasing the bonding strength of the latex.

[0037] The initiator can decompose to produce active free radicals. These free radicals are highly active and can attack styrene and butadiene monomer molecules, activating them and participating in subsequent polymerization reactions, thereby initiating the entire polymerization process.

[0038] The initiator is composed of diisopropylbenzene hydroperoxide and ferrous sulfate in a certain ratio to form a redox initiator system. In this system, ferrous sulfate can reduce the decomposition temperature of diisopropylbenzene hydroperoxide, so that it can also decompose and produce free radicals at low temperatures. These free radicals then initiate the polymerization reaction of the monomer, thereby achieving low-temperature polymerization.

[0039] Ferrous sulfate accounts for 20% of the total mass of the initiator. A lower ferrous sulfate content is not enough to fully accelerate the decomposition of diisopropylbenzene hydroperoxide, thereby affecting the initiation efficiency; a higher content may cause a too fast reaction, making it difficult to control, and even causing safety problems such as explosion.

[0040] The molecular weight regulator is tert-dodecyl mercaptan. In the free radical polymerization reaction, tert-dodecyl mercaptan can undergo a chain transfer reaction with the growing chain radical, thereby limiting the chain length of the polymer, preventing the molecular weight from being too large or too small, and making the molecular weight distribution more uniform.

[0041] The defoamer is a polyether-modified silicone oil emulsion. The polyether-modified silicone oil emulsion has excellent defoaming ability, which can quickly eliminate the foam generated in the production process and inhibit the regeneration of foam, ensuring the smooth progress of the production process, helping to reduce the surface defects of styrene-butadiene latex and improve its appearance quality.

[0042] S3. Preparation for polymerization reaction

[0043] Prepare at least two polymerization kettles and connect them in series into a production line. This can not only improve production efficiency, but also produce products with different properties by controlling the operating conditions of different kettles. Nitrogen is introduced into each polymerization kettle for displacement at least three times to remove the air in the kettle. Subsequently, the polymerization kettle is vacuumed, and the absolute pressure in the kettle is 0.06-0.08MPa.

[0044] The prepared aqueous emulsion is accurately distributed to each polymerization kettle by a metering pump. The amount of each polymerization kettle pumped in is determined according to demand. The agitator in the polymerization kettle is turned on to evenly distribute the aqueous emulsion in the kettle. A refrigerant is introduced into the jacket of the polymerization kettle to cool the kettle body and reduce the temperature in the kettle to a temperature range suitable for polymerization reaction.

[0045] The water phase emulsion in the reactor is distributed to each polymerization reactor by a metering pump, the agitator is turned on, and a refrigerant is introduced into the jacket of the polymerization reactor to cool it down. When the temperature in the reactor drops to 5°C, 30wt% of butadiene and 10wt% of styrene are added to the added water phase emulsion, and the temperature in the reactor is maintained. The two monomers are dispersed in the water phase emulsion and undergo polymerization reaction under the action of the initiator.

[0046] S4, mid-stage polymerization regulation

[0047] During the polymerization reaction, samples were taken and the styrene conversion rate was determined by liquid chromatography. When the conversion rate reached 35-40%, 0.3 wt% of tert-dodecyl mercaptan and 0.5 wt% of electrolyte were added to the added aqueous emulsion. Stirring was continued to ensure that they were evenly dispersed in the emulsion system.

[0048] The purpose of adding tert-dodecyl mercaptan twice is to more finely control the molecular weight distribution and chain structure of the polymer. As the reaction proceeds, the chain length of the polymer gradually increases, and the reaction rate changes accordingly. Adding the molecular weight regulator in batches can help maintain a relatively stable reaction rate.

[0049] The electrolyte is potassium chloride. In emulsion polymerization, the role of potassium chloride is mainly to change the charge state of the emulsion system, to stabilize the latex particles and prevent them from agglomerating, and also to help improve the yield and quality of the polymer. However, if too much potassium chloride is added, the stability of the emulsion may be destroyed, causing the latex particles to agglomerate or precipitate, thereby affecting the polymerization reaction and the performance of the product.

[0050] S5. Termination of polymerization reaction

[0051] During the polymerization reaction, when the conversion rate reaches 85-90%, it means that the reaction is nearly completed and most of the monomers have been converted into polymers. Sodium dimethyldithiocarbamate accounting for 0.2wt% of the added aqueous emulsion is added as a terminator to terminate the polymerization reaction.

[0052] S6. Post-processing

[0053] After the polymerization reaction is completed, the temperature is stopped, and 0.5 wt% of sodium alginate and 0.5 wt% of polyacrylamide are added to adjust the viscosity of the product, and stirring is continued for 0.5 to 1 hour to obtain styrene-butadiene latex.

[0054] Example 2

[0055] Preparation of LL-300B styrene-butadiene latex.

[0056] S1. Add 290 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C;

[0057] S2, 8 parts of emulsifier (compounded by palm sorbitan and sodium rosinate in a certain proportion, the weight ratio of sodium rosinate to palm sorbitan is 1:1), 4 parts of carboxylic acid monomer (compounded by methacrylic acid and acrylic acid in a certain proportion, acrylic acid accounts for 48% of the total weight of carboxylic acid monomer), 1.7 parts of initiator (compounded by diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, ferrous sulfate accounts for 22% of the total weight of initiator), 1.5 parts of tert-dodecyl mercaptan, 0.9 parts of polyether modified silicone oil emulsion are added to deionized water, the above temperature is maintained for 0.5 to 1 hour under stirring and dispersion, heating is stopped, and cooling is performed to room temperature to obtain an aqueous emulsion;

[0058] S3, distribute the aqueous emulsion in the reactor to each polymerization reactor through a metering pump, turn on the agitator and cool it down, when the temperature in the reactor drops to 5°C, add 32wt% of butadiene and 12wt% of styrene to the aqueous emulsion to carry out polymerization reaction;

[0059] S4, when the conversion rate reaches 22-25%, add 0.35wt% of tert-dodecyl mercaptan and 0.8wt% of potassium chloride to the added aqueous phase emulsion, and continue stirring;

[0060] S5. When the conversion rate reaches 85-90%, sodium dimethyldithiocarbamate accounting for 0.3 wt % of the added aqueous emulsion is added to terminate the polymerization reaction;

[0061] S6. After the reaction is completed, stop cooling, add 0.8 wt% of sodium alginate and 0.6 wt% of polyacrylamide to adjust the viscosity of the product, continue stirring for 0.5 to 1 hour, and obtain styrene-butadiene latex.

[0062] Example 3

[0063] Preparation of LL-300C styrene-butadiene latex.

[0064] S1. Add 320 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C;

[0065] S2, add 15 parts of emulsifier (compounded by palm sorbitan and sodium rosinate in a certain proportion, the weight ratio of sodium rosinate to palm sorbitan is 2:3), 6 parts of carboxylic acid monomer (compounded by methacrylic acid and acrylic acid in a certain proportion, acrylic acid accounts for 55% of the total weight of carboxylic acid monomer), 2 parts of initiator (compounded by diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, ferrous sulfate accounts for 25% of the total weight of initiator), 2 parts of tert-dodecyl mercaptan, 1.8 parts of polyether modified silicone oil emulsion into deionized water, maintain the above temperature and stir and disperse for 0.5 to 1 hour, stop heating, cool to room temperature, and obtain an aqueous emulsion;

[0066] S3, distribute the aqueous emulsion in the reactor to each polymerization reactor through a metering pump, turn on the agitator and cool down, when the temperature in the reactor drops to 5°C, add 35wt% of butadiene and 15wt% of styrene to the aqueous emulsion to carry out polymerization reaction;

[0067] S4, when the conversion rate reaches 22-25%, add 0.5wt% of tert-dodecyl mercaptan and 1.5wt% of potassium chloride to the added aqueous phase emulsion, and continue stirring;

[0068] S5. When the conversion rate reaches 85-90%, sodium dimethyldithiocarbamate accounting for 0.5 wt % of the added aqueous emulsion is added to terminate the polymerization reaction;

[0069] S6. After the reaction is completed, stop cooling, add 1.5 wt% of sodium alginate and 1 wt% of polyacrylamide to adjust the viscosity of the product, continue stirring for 0.5 to 1 hour, and obtain styrene-butadiene latex.

[0070] Example 4

[0071] Preparation of LL-400C styrene-butadiene latex.

[0072] S1. Add 280 parts of deionized water to the reactor by mass, start stirring and raise the temperature to 38-45°C;

[0073] S2, 5 parts of emulsifier (compounded by palm sorbitan and sodium rosinate in a certain proportion, the weight ratio of sodium rosinate to palm sorbitan is 3:2), 2.5 parts of carboxylic acid monomer (compounded by methacrylic acid and acrylic acid in a certain proportion, acrylic acid accounts for 50% of the total weight of carboxylic acid monomer), 1.5 parts of initiator (compounded by diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, ferrous sulfate accounts for 23% of the total weight of initiator), 1 part of tert-dodecyl mercaptan, 0.6 parts of polyether modified silicone oil emulsion are added to deionized water, the above temperature is maintained for 0.5 to 1 hour under stirring and dispersion, heating is stopped, and cooling is performed to room temperature to obtain an aqueous emulsion;

[0074] S3, distribute the aqueous emulsion in the reactor to each polymerization reactor through a metering pump, turn on the agitator and cool it down, when the temperature in the reactor drops to 5°C, add 30wt% of butadiene and 10wt% of styrene to the aqueous emulsion to carry out polymerization reaction;

[0075] S4, when the conversion rate reaches 22-25%, add 0.3wt% of tert-dodecyl mercaptan and 0.5wt% of potassium chloride to the added aqueous phase emulsion, and continue stirring;

[0076] S5. When the conversion rate reaches 85-90%, sodium dimethyldithiocarbamate accounting for 0.2 wt % of the added aqueous emulsion is added to terminate the polymerization reaction;

[0077] S6. After the reaction is completed, stop cooling, add 0.5 wt% of sodium alginate and 0.5 wt% of polyacrylamide to adjust the viscosity of the product, continue stirring for 0.5 to 1 hour, and obtain styrene-butadiene latex.

[0078] Example 5

[0079] Preparation of LL-500C styrene-butadiene latex.

[0080] S1. Add 290 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C;

[0081] S2, 8 parts of emulsifier (compounded by palm sorbitan and sodium rosinate in a certain proportion, the weight ratio of sodium rosinate to palm sorbitan is 3:2), 4 parts of carboxylic acid monomer (compounded by methacrylic acid and acrylic acid in a certain proportion, acrylic acid accounts for 50% of the total weight of carboxylic acid monomer), 1.7 parts of initiator (compounded by diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, ferrous sulfate accounts for 25% of the total weight of initiator), 1.5 parts of tert-dodecyl mercaptan, 0.9 parts of polyether modified silicone oil emulsion are added to deionized water, the above temperature is maintained for 0.5 to 1 hour of stirring and dispersion, heating is stopped, and cooling is performed to room temperature to obtain an aqueous emulsion;

[0082] S3, distribute the aqueous emulsion in the reactor to each polymerization reactor through a metering pump, turn on the agitator and cool it down, when the temperature in the reactor drops to 5°C, add 32wt% of butadiene and 12wt% of styrene to the aqueous emulsion to carry out polymerization reaction;

[0083] S4, when the conversion rate reaches 22-25%, add 0.35wt% of tert-dodecyl mercaptan and 0.8wt% of potassium chloride to the added aqueous phase emulsion, and continue stirring;

[0084] S5. When the conversion rate reaches 85-90%, sodium dimethyldithiocarbamate accounting for 0.3 wt % of the added aqueous emulsion is added to terminate the polymerization reaction;

[0085] S6. After the reaction is completed, stop cooling, add 0.8 wt% of sodium alginate and 0.6 wt% of polyacrylamide to adjust the viscosity of the product, continue stirring for 0.5 to 1 hour, and obtain styrene-butadiene latex.

[0086] Example 6

[0087] Preparation of LL-600C styrene-butadiene latex.

[0088] S1. Add 320 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C;

[0089] S2, add 15 parts of emulsifier (compounded by palm sorbitan and sodium rosinate in a certain proportion, the weight ratio of sodium rosinate to palm sorbitan is 3:2), 6 parts of carboxylic acid monomer (compounded by methacrylic acid and acrylic acid in a certain proportion, acrylic acid accounts for 50% of the total weight of carboxylic acid monomer), 2 parts of initiator (compounded by diisopropylbenzene hydroperoxide and ferrous sulfate in a certain proportion, ferrous sulfate accounts for 23% of the total weight of initiator), 2 parts of tert-dodecyl mercaptan, 1.8 parts of polyether modified silicone oil emulsion into deionized water, maintain the above temperature and stir and disperse for 0.5 to 1h, stop heating, cool to room temperature, and obtain an aqueous emulsion;

[0090] S3, distribute the aqueous emulsion in the reactor to each polymerization reactor through a metering pump, turn on the agitator and cool down, when the temperature in the reactor drops to 5°C, add 35wt% of butadiene and 15wt% of styrene to the aqueous emulsion to carry out polymerization reaction;

[0091] S4, when the conversion rate reaches 22-25%, add 0.5wt% of tert-dodecyl mercaptan and 1.5wt% of potassium chloride to the added aqueous phase emulsion, and continue stirring;

[0092] S5. When the conversion rate reaches 85-90%, sodium dimethyldithiocarbamate accounting for 0.5 wt % of the added aqueous emulsion is added to terminate the polymerization reaction;

[0093] S6. After the reaction is completed, stop cooling, add 1.5 wt% of sodium alginate and 1 wt% of polyacrylamide to adjust the viscosity of the product, continue stirring for 0.5 to 1 hour, and obtain styrene-butadiene latex.

[0094] In step S6 of the above-mentioned embodiments 1-6, the prepared styrene-butadiene latex needs to be degassed to achieve the purpose of recovering unreacted products and reducing volatile organic compounds.

[0095] The styrene butadiene latex flowing out of each polymerization reactor is collected together and temporarily stored in a buffer tank. During the degassing process, the styrene butadiene latex is processed in two flash evaporators in turn, and the volatile components in the styrene butadiene latex are quickly vaporized and separated by reducing the pressure.

[0096] In the first flash evaporator, the internal temperature is maintained at 25-30°C, and the pressure is controlled at 0.02-0.05MPa. Since butadiene has a low boiling point and high volatility under this temperature and pressure condition, most of the butadiene can be effectively removed at this stage. The styrene-butadiene latex that has undergone preliminary degassing enters the second flash evaporator. The internal temperature of the second flash evaporator is maintained at 28-30°C, slightly higher than that of the first flash evaporator, and the pressure is further reduced to 0.01-0.02MPa. Since the pressure of the second flash evaporator is lower, the vaporization of butadiene is easier, so that most of the butadiene can be removed. After the evaporated butadiene is condensed to remove nitrogen, it is put back into the production process as a raw material to improve resource utilization.

[0097] The styrene butadiene latex from which butadiene has been removed enters the stripping tower to remove the unreacted styrene. The bottom of the stripping tower is heated by steam, the pressure at the top of the tower is 0.01-0.03 MPa, and the temperature at the top of the tower is maintained at 48-53°C. Styrene and part of the water vapor are evaporated from the top of the stripping tower. After condensation, the water is separated from the styrene, and the styrene is put back into the production process as a raw material.

[0098] The addition amount of each component in Examples 1-6 was recorded and Table 1 was plotted:

[0099]

[0100] After degassing, the styrene-butadiene latex obtained in Examples 1-6 was subjected to performance testing and the test results were recorded. The specific data are shown in Table 2:

[0101]

[0102] After accurately controlling the selection and dosage of each component, the performance of the styrene-butadiene latex prepared by the preparation method can be further significantly improved. The viscosity of the styrene-butadiene latex is ≥483mpas / 25°C, and the average particle size is 281.5nm (the average value of Examples 1-6), which is of great significance in improving the adhesion, wear resistance and anti-aging properties of asphalt during asphalt modification.

[0103] According to the embodiments of the present invention as described above, these embodiments do not describe all the details in detail, nor do they limit the invention to specific embodiments. Obviously, many modifications and changes can be made based on the above description. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can make good use of the present invention and the modified use based on the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a tackified environmentally friendly styrene-butadiene latex, It is characterized in that The steps include: S1. Add 280-320 parts of deionized water by mass into the reactor, start stirring and raise the temperature to 38-45°C; S2, adding 5 to 15 parts of emulsifier, 2.5 to 6 parts of carboxylic acid monomer, 1.5 to 2 parts of initiator, 1 to 2 parts of molecular weight regulator, and 0.6 to 1.8 parts of defoamer into deionized water, keeping warm and stirring and dispersing for 0.5 to 1.5 hours, stopping heating, cooling to room temperature, and obtaining an aqueous emulsion; The emulsifier is composed of palm sorbitan and sodium rosinate in a proportion, and the weight ratio of the sodium rosinate to palm sorbitan is 3:1; The carboxylic acid monomer is composed of methacrylic acid and acrylic acid in a certain proportion, and the acrylic acid accounts for 45-55% of the total weight of the carboxylic acid monomer; S3, nitrogen was introduced into the polymerization kettle for replacement three times and vacuum was drawn, the aqueous emulsion in the reaction kettle was sent to the polymerization kettle by a metering pump, the agitator was turned on, and a refrigerant was introduced into the jacket of the polymerization kettle to cool it down. When the temperature in the kettle dropped to 5°C, butadiene accounting for 30-35wt% of the added aqueous emulsion and styrene accounting for 10-15wt% of the added aqueous emulsion were added, the temperature in the kettle was maintained, and the polymerization reaction was carried out; S4, taking samples, determining the styrene conversion rate by liquid chromatography, when the conversion rate reaches 35-40%, adding 0.3-0.5wt% of the molecular weight regulator and 0.5-1.5wt% of the electrolyte to the added aqueous emulsion, and continuing stirring; S5. When the conversion rate reaches 85-90%, adding a terminator accounting for 0.2-0.5 wt % of the added aqueous emulsion to terminate the polymerization reaction; S6. After the reaction is completed, stop cooling, add 0.5-1.5wt% of sodium alginate and 0.5-1wt% of polyacrylamide, respectively, and stir for 0.5-1h to obtain styrene-butadiene latex.

2. The preparation method according to claim 1, Features: In step S6, the styrene butadiene latex obtained by the polymerization kettle is transported to a buffer tank, the styrene butadiene latex coming out of the buffer tank is recovered by a flash evaporator to remove incompletely reacted butadiene, the styrene butadiene latex from which butadiene is removed enters a stripping tower to remove incompletely reacted styrene, the styrene butadiene latex from which styrene is removed flows out from the bottom of the stripping tower and is then stored in a finished product tank.

3. The preparation method according to claim 1, Features: The initiator is composed of diisopropylbenzene hydroperoxide and ferrous sulfate mixed in proportion, and the ferrous sulfate accounts for 20-25% of the total mass of the initiator.

4. The preparation method according to claim 1, Features: The molecular weight regulator is tert-dodecyl mercaptan.

5. The preparation method according to claim 1, Features: The defoamer is polyether modified silicone oil emulsion.

6. The preparation method according to claim 1, Features: The electrolyte is potassium chloride.

7. The preparation method according to claim 1, Features: The terminator is sodium dimethyldithiocarbamate.