Moisture-proof and antibacterial bamboo charcoal bristle and preparation method thereof and application in toothbrush

By using bamboo charcoal powder with mesoporous titanium dioxide on the surface loaded in the toothbrush silk, and modified with quaternary ammonium salts and silane coupling agents, a functional additive with antibacterial and toughening effects is formed. The problems of antibacterial agent dissolution and material elasticity are solved, and the effects of moisture-proof and anti-bacterial and anti-hair effects are achieved.

CN118563448BActive Publication Date: 2024-11-19SHANTOU YIN JIE DAILY PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058003.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing antibacterial agents are added directly to the polymer, which will continue to dissolve during the use of the toothbrush, resulting in a decrease in the antibacterial properties of the material. The mechanical properties of the polymer, such as elasticity, are prone to hair reversal.

Method used

Bamboo charcoal powder is used as a carrier to prepare bamboo charcoal powder with mesoporous titanium dioxide surface loaded by ultrasonic assisted template method, and organically modified with quaternary ammonium cationic surfactant and silane coupling agent to form functional additives and combine with ethylene- The octene copolymer is reacted with hydroxypropyl acrylate to form a polymer with rigid dispersed phase particles, and is added to polybutylene terephthalate to enhance the impact toughness and antibacterial properties of the material through cross-linking reaction.

Benefits of technology

It effectively improves the impact toughness and antibacterial properties of the material, reduces the dissolution problem of functional additives, maintains the good resilience of the polymer, avoids the phenomenon of hair reflux, and has excellent moisture-proof and sterilization and antibacterial properties in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a moisture-proof and antibacterial bamboo charcoal bristle filament, a preparation method thereof and an application thereof in a toothbrush, and relates to the technical field of daily necessities. The moisture-proof and antibacterial bamboo charcoal bristle filament preparation method of the invention comprises the following steps: adding polybutylene terephthalate and a functional additive to a twin-screw extruder for melt extrusion and granulation to obtain a master batch; adding the master batch to a melt spinning machine for melt spinning and cooling and forming to obtain a moisture-proof and antibacterial bamboo charcoal bristle filament; the functional additive prepared in the present application is added to polybutylene terephthalate for melt grafting reaction, which not only improves the moisture-proof and antibacterial properties of the material, but also gives the polybutylene terephthalate good mechanical properties; the moisture-proof and antibacterial bamboo charcoal bristle filament is applied in a toothbrush and has excellent anti-hair falling and antibacterial moisture resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of daily necessities, and in particular to moisture-proof and antibacterial bamboo charcoal bristle filaments, a preparation method thereof, and application in toothbrushes. Background Art

[0002] The oral cavity and teeth are one of the main portals for bacteria to invade the human body. As a special tool for cleaning the oral cavity, toothbrushes play a great role in ensuring oral hygiene and preventing oral diseases. Toothbrushes are in a humid environment for a long time during use, and various microorganisms attached to the toothbrush filaments multiply rapidly in a humid and warm environment. Therefore, as the toothbrush head that directly contacts the oral cavity, the toothbrush filaments need to use antibacterial materials to make the toothbrush head antibacterial, reduce the number of microorganisms carried on the surface of the toothbrush head, and thus reduce the risk of infection caused by microorganisms on the surface of the toothbrush to the teeth or gums during brushing.

[0003] The toothbrush bristles on the market are generally made of nylon, PBT, and PP as raw materials. Among them, PBT (polybutylene terephthalate) is a crystalline linear saturated polyester obtained by polycondensation of terephthalic acid and 1,4-butanediol. Compared with nylon and PP bristles, PBT has the advantages of not easy to fall, low water absorption, low wear rate, and high resilience. In order to improve the antibacterial properties of toothbrush filaments, many toothbrush filaments are currently made by adding antibacterial agents to the raw materials of bristles. Antibacterial agents for plastics are generally divided into the following categories: inorganic antibacterial agents, organic antibacterial agents, organic-inorganic composite antibacterial agents, polymer antibacterial agents, and natural antibacterial agents. Antibacterial agents are directly added to polymers and will continue to dissolve during the use of toothbrushes, which not only reduces the antibacterial properties of the material, but also reduces the mechanical properties of the polymer itself, such as elasticity, due to the addition of antibacterial agents, and is prone to falling hair. Summary of the invention

[0004] The purpose of the present invention is to provide a moisture-proof and antibacterial bamboo charcoal bristle and a preparation method thereof and an application in a toothbrush, so as to solve the following technical problems: the existing antibacterial agent is directly added to a polymer and will be continuously dissolved during the use of the toothbrush, which not only leads to a decrease in the antibacterial property of the material, but also reduces the mechanical properties of the polymer itself, such as elasticity.

[0005] The purpose of the present invention can be achieved by the following technical solution: A method for preparing moisture-proof and antibacterial bamboo charcoal bristles, comprising the following steps:

[0006] S1: adding polybutylene terephthalate and functional additives into a twin-screw extruder for melt extrusion and granulation to obtain a masterbatch;

[0007] S2: adding the masterbatch to a melt spinning machine for melt spinning and cooling to form, thereby obtaining moisture-proof and antibacterial bamboo charcoal bristle filaments; the preparation method of the functional additive comprises the following steps: A1: adding tetrabutyl titanate and anhydrous ethanol to a reactor and dispersing them evenly, adding a pore-forming agent solution and bamboo charcoal powder to a reactor and dispersing them evenly, aging at room temperature for 24-32 hours, filtering, drying, and calcining to obtain component one; A2: in a nitrogen atmosphere, adding tetraoctylammonium bromide and toluene to a reactor and dispersing them evenly, adding component one and dispersing them evenly, adding isocyanate propyl triethoxysilane, controlling the temperature to 70-80°C, and keeping the reaction temperature for 24 hours. -48h, washed with xylene and dried to obtain component two; A3: In a nitrogen atmosphere, add component two and toluene into the reactor and disperse evenly, add hydroxypropyl acrylate, control the temperature at 85-95°C, keep warm for 24-36h under stirring conditions, add ε-caprolactam, control the temperature at 70-80°C, keep warm for 1-3h, centrifuge, wash with toluene, and dry to obtain component three; A4: Stir ethylene-octene copolymer, glycidyl methacrylate, component three, and diisopropylbenzene peroxide evenly, melt, extrude, and granulate in a twin-screw extruder to obtain the functional additive epoxidized ethylene-octene copolymer.

[0008] As a further scheme of the present invention: the preparation method of the bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying the bamboo at 100-180°C, pre-carbonizing at 180-280°C, carbonizing at 280-450°C, and firing at 450-1200°C under a nitrogen atmosphere; subjecting the carbonized material to water vapor activation treatment at 1000°C, and grinding to obtain food-grade bamboo charcoal powder of 0.1-0.3um.

[0009] As a further solution of the present invention: the masterbatch contains 10-20wt% of functional additives.

[0010] As a further solution of the present invention: the pore-forming agent solution in A1 is prepared by mixing 1 g of hexadecyltrimethylammonium bromide, 8-10 mL of anhydrous ethanol, and 1.5-2 mL of deionized water, adding concentrated hydrochloric acid to adjust the pH to 2-3, and stirring at 30-35° C. for 15-30 min; the addition ratio of tetrabutyl titanate, anhydrous ethanol, pore-forming agent solution, and bamboo charcoal powder in A1 is 10 mL: 40-50 mL: 10-15 mL: 5-15 g.

[0011] As a further embodiment of the present invention, the addition ratio of tetraoctylammonium bromide, toluene, component 1, and isocyanatepropyltriethoxysilane in A2 is 0.2-0.3 g: 30-50 mL: 1 g: 1-2 mL.

[0012] As a further solution of the present invention: the addition ratio of component II, toluene, hydroxypropyl acrylate and ε-caprolactam in A3 is 1 g: 30-50 mL: 0.2-0.4 g: 0.5-0.7 g.

[0013] As a further solution of the present invention: in A4, the addition ratio of ethylene-octene copolymer, glycidyl methacrylate, component three, and dicumyl peroxide is 10g: 0.1-0.5g: 8-12g: 0.4-0.6g.

[0014] As a further scheme of the present invention: the process parameters of the twin screw extruder in S1 are set to: 200-210°C for zone 1, 210-220°C for zone 2, 230-235°C for zone 3, 240-250°C for zone 4, 250-260°C for zone 5, and the speed of the twin screw extruder is 160-180rpm; the process parameters of the twin screw extruder in A4 are set to: 160-170°C for zone 1, 160-170°C for zone 2, 160-170°C for zone 3, 170-180°C for zone 4, 170-180°C for zone 5, 170-180°C for zone 6, 170-180°C for zone 7, and the screw speed is 50-60rpm.

[0015] As a further solution of the present invention: the process parameters of the melt spinning machine are set as follows: temperature 230-240° C., draft ratio 4.80-4.95.

[0016] A moisture-proof and antibacterial bamboo charcoal brush bristle filament is made by any one of the above-mentioned preparation methods of the moisture-proof and antibacterial bamboo charcoal brush bristle filament.

[0017] An application of the moisture-proof and antibacterial bamboo charcoal bristles in a toothbrush.

[0018] The beneficial effects of the present invention are as follows: (1) The present invention utilizes bamboo charcoal powder, which has the characteristics of large specific surface area, low cost and non-toxicity, as a carrier; using hexadecyltrimethylammonium bromide as a pore-forming agent, tetrabutyl titanate as a titanium source and bamboo charcoal powder as a carrier, bamboo charcoal powder with mesoporous titanium dioxide loaded on the surface is successfully prepared by an ultrasonic-assisted template method; the present invention utilizes quaternary ammonium salt cationic surfactant tetraoctylammonium bromide to organically modify the bamboo charcoal powder to improve the dispersion uniformity of the bamboo charcoal powder in toluene, and utilizes a silane coupling agent to organically modify the bamboo charcoal powder to obtain component two; the present invention utilizes hydroxypropyl acrylate to react with part of the isocyanate groups on the surface of component two to obtain bamboo charcoal powder with carbon-carbon double bonds grafted on the surface, and during the preparation process, ε-caprolactam is used as a capping agent to cap the remaining isocyanate groups on the surface of the bamboo charcoal powder to obtain component three; the present invention utilizes the double bonds of component three to graft with ethylene-octene copolymer, and utilizes glycidyl methacrylate to graft epoxy groups on the ethylene-octene copolymer to obtain a functional additive. The functional additive prepared in the present application is actually a polymer containing rigid dispersed phase particles, which is added to a high molecular polymer matrix to improve the impact toughness of the material, with bamboo charcoal powder loaded with mesoporous titanium dioxide as the core and ethylene-octene copolymer elastomer as the shell.

[0019] The prepared functional additive is added to polybutylene terephthalate, which exhibits a synergistic toughening effect. The functional additive and polybutylene terephthalate are melt-reacted in a twin-screw extruder, that is, a volume expansion reaction that is beneficial to toughening is generated. During the melt reaction, the functional additive is cross-linked with the terminal carboxyl group and the terminal hydroxyl group of the polybutylene terephthalate through the epoxy group, and the functional additive is chemically bonded to the polybutylene terephthalate molecular chain. The bamboo charcoal powder loaded with mesoporous titanium dioxide on the functional additive prepared in the present application is organically cross-linked with polybutylene terephthalate through ethylene-octene copolymer, and the ε-caprolactam blocked with isocyanate groups grafted on the surface of the mesoporous titanium dioxide is unblocked during the melting process of the twin-screw extruder, the isocyanate groups further increase the cross-linking, the entanglement between the molecular chains is enhanced, the interfacial tension is weakened, the compatibility is improved, and the material forms a three-dimensional network structure, which not only greatly reduces the problem of dissolution of the functional additive; but also the functional additive and polybutylene terephthalate are cross-linked to reduce the interfacial effect, effectively reducing the problem of reduced mechanical properties of polybutylene terephthalate caused by the addition of the functional additive, so that the polybutylene terephthalate maintains good resilience and avoids the occurrence of the inverted hair phenomenon.

[0020] (2) In the process of preparing the functional additive of the present application, mesoporous titanium dioxide is first loaded on the surface of bamboo charcoal powder. The bamboo charcoal powder loaded with mesoporous titanium dioxide has a large specific surface area, which makes the material have more active sites and hydroxyl radicals. When the functional additive is added to polybutylene terephthalate, it not only gives the material good antibacterial properties. The bamboo charcoal powder loaded with mesoporous titanium dioxide on the surface of the functional additive has good crystallization properties to promote the separation of photogenerated electrons and holes, but also in a humid environment, the water adsorbed on the surface of the material is oxidized into ·OH. The generated ·OH will attack the unsaturated bonds of organic matter or extract its H atoms, resulting in peptide chain breakage and sugar depolymerization, thereby causing protein mutation and lipid decomposition, thereby achieving photocatalytic sterilization; giving the material excellent moisture-proof properties and bactericidal and antibacterial properties. DETAILED DESCRIPTION

[0021] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] The preparation method of the functional additive comprises the following steps:

[0024] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0025] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 40mL anhydrous ethanol were added to the reactor and dispersed evenly, 10mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 24h, filtered, dried at 100°C for 6h, and calcined at 500°C for 2h to obtain component 1;

[0026] A3: In a nitrogen atmosphere, add 2g of tetraoctylammonium bromide and 300mL of toluene into a reaction kettle and disperse them evenly, add 10g of component 1 and disperse them evenly, add 10mL of isocyanatepropyltriethoxysilane, control the temperature at 70°C, keep the reaction warm for 24h, wash with xylene, and dry to obtain component 2;

[0027] A4: In a nitrogen atmosphere, 10 g of component 2 and 300 mL of toluene were added to a reaction kettle and dispersed evenly. 2 g of hydroxypropyl acrylate was added, the temperature was controlled at 85°C, and the mixture was kept warm for 24 h under stirring. 5 g of ε-caprolactam was added, the temperature was controlled at 70°C, and the mixture was kept warm for 1 h. The mixture was centrifuged, washed with toluene, and dried to obtain component 3.

[0028] A5: 10g of ethylene-octene copolymer (POE, 8200), 0.1g of glycidyl methacrylate, 10g of component three and 0.4g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0029] Example 2

[0030] The preparation method of the functional additive comprises the following steps:

[0031] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0032] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 45mL anhydrous ethanol were added to the reactor and dispersed evenly, 12mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 27h, filtered, dried at 100°C for 8h, and calcined at 500°C for 2h to obtain component 1;

[0033] A3: In a nitrogen atmosphere, 2.5 g of tetraoctylammonium bromide and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of component 1 was added and dispersed evenly, 15 mL of isocyanatepropyltriethoxysilane was added, the temperature was controlled at 75 ° C, the reaction was kept warm for 36 hours, washed with xylene, and dried to obtain component 2;

[0034] A4: In a nitrogen atmosphere, 10 g of component 2 and 400 mL of toluene were added to a reaction kettle and dispersed evenly. 3 g of hydroxypropyl acrylate was added, the temperature was controlled at 90°C, and the mixture was kept warm for 30 h under stirring. 6 g of ε-caprolactam was added, the temperature was controlled at 75°C, and the mixture was kept warm for 2 h. The mixture was centrifuged, washed with toluene, and dried to obtain component 3.

[0035] A5: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of component three and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0036] Example 3

[0037] The preparation method of the functional additive comprises the following steps:

[0038] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0039] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 50mL anhydrous ethanol were added to the reactor and dispersed evenly, 15mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 32h, filtered, dried at 100°C for 9h, and calcined at 500°C for 2h to obtain component 1;

[0040] A3: In a nitrogen atmosphere, 3 g of tetraoctylammonium bromide and 500 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of component 1 was added and dispersed evenly, 20 mL of isocyanatepropyltriethoxysilane was added, the temperature was controlled at 80°C, the reaction was kept warm for 48 hours, washed with xylene, and dried to obtain component 2;

[0041] A4: In a nitrogen atmosphere, 10 g of component 2 and 500 mL of toluene were added to a reaction kettle and dispersed evenly. 4 g of hydroxypropyl acrylate was added, the temperature was controlled at 95°C, and the mixture was kept warm for 36 h under stirring. 7 g of ε-caprolactam was added, the temperature was controlled at 80°C, and the mixture was kept warm for 3 h. The mixture was centrifuged, washed with toluene, and dried to obtain component 3.

[0042] A5: 10g of ethylene-octene copolymer (POE, 8200), 0.5g of glycidyl methacrylate, 12g of component three and 0.6g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0043] Example 4

[0044] A method for preparing moisture-proof and antibacterial bamboo charcoal bristles comprises the following steps:

[0045] S1: 80 g of polybutylene terephthalate (brand number L2100) and 20 g of the functional additive prepared in Example 1 were added to a twin-screw extruder for melt extrusion (zone 1 210° C., zone 2 220° C., zone 3 230° C., zone 4 240° C., zone 5 250° C., twin-screw extruder speed: 180 rpm), and granulated to obtain a masterbatch;

[0046] S2: adding the masterbatch into a melt spinning machine for melt spinning (temperature 230-240°C, draft ratio 4.80-4.95), cooling and forming, and obtaining moisture-proof and antibacterial bamboo charcoal bristle filaments.

[0047] Example 5

[0048] Compared with Example 4, Example 5 is only that the functional auxiliary agent prepared in Example 1 added in Example 4 is replaced with the functional auxiliary agent prepared in Example 2 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0049] Example 6

[0050] Compared with Example 4, Example 6 is different in that only the functional additive prepared in Example 1 added in Example 4 is replaced with the functional additive prepared in Example 3 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0051] Comparative Example 1

[0052] The preparation method of the functional additive comprises the following steps:

[0053] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0054] A2: 20 mL of anhydrous ethanol and 4 mL of deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30 min to obtain a solution; 10 mL of tetrabutyl titanate and 45 mL of anhydrous ethanol were added to the reaction kettle and dispersed evenly, 12 mL of the solution and 10 g of bamboo charcoal powder were added to the reaction kettle and dispersed evenly, aged at room temperature for 27 h, filtered, dried at 100°C for 8 h, and calcined at 500°C for 2 h to obtain component 1;

[0055] A2: In a nitrogen atmosphere, 2.5 g of tetraoctylammonium bromide and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of bamboo charcoal powder was added and dispersed evenly, 15 mL of isocyanatepropyltriethoxysilane was added, the temperature was controlled at 75°C, the reaction was kept warm for 36 hours, washed with xylene, and dried to obtain component 2;

[0056] A3: In a nitrogen atmosphere, 10 g of component 2 and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 3 g of hydroxypropyl acrylate was added, the temperature was controlled at 90°C, and the mixture was kept warm for 30 h under stirring, 6 g of ε-caprolactam was added, the temperature was controlled at 75°C, and the mixture was kept warm for 2 h, centrifuged, washed with toluene, and dried to obtain component 3;

[0057] A4: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of component three and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0058] Comparative Example 2

[0059] The preparation method of the functional additive comprises the following steps:

[0060] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0061] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 45mL anhydrous ethanol were added to the reactor and dispersed evenly, 12mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 27h, filtered, dried at 100°C for 8h, and calcined at 500°C for 2h to obtain component 1;

[0062] A3: In a nitrogen atmosphere, 2.5 g of tetraoctylammonium bromide and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of component 1 was added and dispersed evenly, 15 mL of vinyltriethoxysilane was added, the temperature was controlled at 75 ° C, the reaction was kept warm for 36 hours, washed with xylene, and dried to obtain component 2;

[0063] A4: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of component 2, and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded, and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0064] Comparative Example 3

[0065] The preparation method of the functional additive comprises the following steps:

[0066] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0067] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 45mL anhydrous ethanol were added to the reactor and dispersed evenly, 12mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 27h, filtered, dried at 100°C for 8h, and calcined at 500°C for 2h to obtain component 1;

[0068] A3: In a nitrogen atmosphere, 2.5 g of tetraoctylammonium bromide and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of component 1 was added and dispersed evenly, 15 mL of isocyanatepropyltriethoxysilane was added, the temperature was controlled at 75 ° C, the reaction was kept warm for 36 hours, washed with xylene, and dried to obtain component 2;

[0069] A4: In a nitrogen atmosphere, 10 g of component 2 and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 3 g of hydroxypropyl acrylate was added, the temperature was controlled at 90°C, and the mixture was kept warm for 30 h under stirring conditions, centrifuged, washed with toluene, and dried to obtain component 3;

[0070] A5: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of component three and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0071] Comparative Example 4

[0072] The preparation method of the functional additive comprises the following steps:

[0073] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0074] A2: 2g hexadecyltrimethylammonium bromide, 20mL anhydrous ethanol and 4mL deionized water were mixed, concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was stirred at 35°C for 30min to obtain a pore-forming agent solution; 10mL tetrabutyl titanate and 45mL anhydrous ethanol were added to the reactor and dispersed evenly, 12mL pore-forming agent solution and 10g bamboo charcoal powder were added to the reactor and dispersed evenly, aged at room temperature for 27h, filtered, dried at 100°C for 8h, and calcined at 500°C for 2h to obtain component 1;

[0075] A3: In a nitrogen atmosphere, 2.5 g of tetraoctylammonium bromide and 400 mL of toluene were added to a reaction kettle and dispersed evenly, 10 g of component 1 was added and dispersed evenly, 15 mL of isocyanatepropyltriethoxysilane was added, the temperature was controlled at 75 ° C, the reaction was kept warm for 36 hours, washed with xylene, and dried to obtain component 2;

[0076] A4: In a nitrogen atmosphere, 10 g of component 2 and 400 mL of toluene were added to a reactor and dispersed evenly, and 6 g of ε-caprolactam was added. The temperature was controlled at 75°C, and the reaction was kept warm for 2 h. The mixture was centrifuged, washed with toluene, and dried to obtain component 3.

[0077] A5: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of component three and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0078] Comparative Example 5

[0079] The preparation method of the functional additive comprises the following steps:

[0080] A1: The preparation method of bamboo charcoal powder comprises the following steps: controlling the heating rate to 10°C / min, drying bamboo at 100°C, pre-carbonizing at 280°C, carbonizing at 450°C, and sintering at 1200°C under a nitrogen atmosphere; subjecting the carbonized material to steam activation treatment at 1000°C, and grinding to obtain 0.3um food-grade bamboo charcoal powder;

[0081] A2: 10g of ethylene-octene copolymer (POE, 8200), 0.3g of glycidyl methacrylate, 10g of bamboo charcoal powder and 0.5g of dicumyl peroxide were stirred evenly, melted in a twin-screw extruder (the process parameters of the twin-screw extruder were set as follows: zone 1 170°C, zone 2 170°C, zone 3 170°C, zone 4 180°C, zone 5 180°C, zone 6 180°C, zone 7 180°C, screw speed 60rpm), extruded and granulated to obtain a functional additive epoxidized ethylene-octene copolymer.

[0082] Comparative Example 6

[0083] Compared with Example 4, Comparative Example 6 is that only the functional auxiliary agent prepared in Example 1 added in Example 4 is replaced with the functional auxiliary agent prepared in Comparative Example 1 in equal amount, and the other components and preparation method are completely consistent with Example 4.

[0084] Comparative Example 7

[0085] Compared with Example 4, Comparative Example 7 is that only the functional additive prepared in Example 1 added in Example 4 is replaced with the functional additive prepared in Comparative Example 2 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0086] Comparative Example 8

[0087] Compared with Example 4, Comparative Example 8 is that only the functional additive prepared in Example 1 added in Example 4 is replaced with the functional additive prepared in Comparative Example 3 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0088] Comparative Example 9

[0089] Compared with Example 4, Comparative Example 9 is that only the functional additive prepared in Example 1 added in Example 4 is replaced with the functional additive prepared in Comparative Example 4 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0090] Comparative Example 10

[0091] Compared with Example 4, Comparative Example 10 is that only the functional additive prepared in Example 1 added in Example 4 is replaced with the functional additive prepared in Comparative Example 5 in equal amount, and the other components and preparation method are completely the same as those in Example 4.

[0092] Performance Testing

[0093] (1) Antibacterial rate: Tested according to Appendix B of GB / T 21510-2008 “Test methods for antibacterial properties of nano-inorganic materials”; 10 7 cfu / mL bacterial solution, 1.00g bristle and 5mL bacterial solution were added to a shaking flask, and the live bacteria were counted after curing at 25℃ for 10h, and the sterilization rate was calculated; in addition, the bristle was immersed in 10wt% sucrose solution for 3min every day and then rinsed with tap water for 1min, and the sterilization rate was calculated after 90 days; the test results are shown in Table 1;

[0094]

[0095] It can be seen from Table 1 that the bristle filaments prepared in the present application have good antibacterial properties, and after multiple washings, they still maintain good antibacterial properties, indicating that the functional additives prepared in the present application have high interfacial bonding strength with the polyester matrix, and the functional additives are not easily dissolved during use.

[0096] (2) Single filament bending recovery rate: According to the relevant content of GB / T 19342-2013 "Toothbrush" on the complete recovery rate of single filament bristles, the bristles were placed in the hole of a metal plate (hole diameter 1.5 mm), and the bristles were immersed in (50±2)℃ water for 2 min and then taken out. They were then immersed in (20±2)℃ water for 0.5 min and then taken out. Finally, they were immersed in (20±2)℃ water for 15 min. After taking out, the angle θ was measured and the single filament bending recovery rate K (%) was calculated; K (%) = θ / 180×100

[0097] Where, K-single wire bending recovery rate, %; θ-bending angle, °; the test results are shown in Table 2;

[0098]

[0099] It can be seen from Table 2 that the bristle filaments prepared in the present application have a good bending recovery rate and are applied to toothbrush bristles so that the toothbrush can rebound and recover quickly after bending during use, thereby increasing the service life of the toothbrush.

[0100] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing moisture-proof and antibacterial bamboo charcoal bristles, It is characterized in that The steps include: S1: adding polybutylene terephthalate and functional additives into a twin-screw extruder for melt extrusion and granulation to obtain a masterbatch; S2: adding the masterbatch into a melt spinning machine for melt spinning and cooling to form moisture-proof and antibacterial bamboo charcoal bristle filaments; The preparation method of the functional additive comprises the following steps: A1: Tetrabutyl titanate and anhydrous ethanol are added to a reaction kettle and dispersed evenly, pore-forming agent solution and bamboo charcoal powder are added to the reaction kettle and dispersed evenly, aged at room temperature for 24-32 hours, filtered, dried, and calcined to obtain component 1; A2: In a nitrogen atmosphere, tetraoctylammonium bromide and toluene are added to a reaction kettle and dispersed evenly, component 1 is added and dispersed evenly, isocyanate propyl triethoxysilane is added, the temperature is controlled at 70-80°C, the reaction is kept warm for 24-48h, washed with xylene, and dried to obtain component 2; A3: In a nitrogen atmosphere, add component 2 and toluene into a reaction kettle and disperse them evenly, add hydroxypropyl acrylate, control the temperature at 85-95°C, keep warm for 24-36 hours under stirring, add ε-caprolactam, control the temperature at 70-80°C, keep warm for 1-3 hours, centrifuge, wash with toluene, and dry to obtain component 3; A4: Ethylene-octene copolymer, glycidyl methacrylate, component three and dicumyl peroxide are uniformly stirred, melted, extruded and granulated in a twin-screw extruder to obtain a functional additive epoxidized ethylene-octene copolymer; The pore-forming agent solution in A1 is prepared by mixing 1 g of hexadecyltrimethylammonium bromide, 8-10 mL of anhydrous ethanol, and 1.5-2 mL of deionized water, adding concentrated hydrochloric acid to adjust the pH to 2-3, and stirring at 30-35° C. for 15-30 minutes; the addition ratio of tetrabutyl titanate, anhydrous ethanol, pore-forming agent solution, and bamboo charcoal powder in A1 is 10 mL: 40-50 mL: 10-15 mL: 5-15 g.

2. A method for preparing moisture-proof and antibacterial bamboo charcoal bristles according to claim 1, It is characterized in that The masterbatch contains 10-20wt% of functional additives.

3. A method for preparing moisture-proof and antibacterial bamboo charcoal brush bristles according to claim 1, It is characterized in that The addition ratio of tetraoctylammonium bromide, toluene, component one, and isocyanatepropyltriethoxysilane in A2 is 0.2-0.3 g: 30-50 mL: 1 g: 1-2 mL.

4. A method for preparing moisture-proof and antibacterial bamboo charcoal bristles according to claim 1, It is characterized in that The addition ratio of component II, toluene, hydroxypropyl acrylate and ε-caprolactam in A3 is 1g:30-50mL:0.2-0.4g:0.5-0.7g.

5. A method for preparing moisture-proof and antibacterial bamboo charcoal bristles according to claim 1, It is characterized in that In A4, the addition ratio of ethylene-octene copolymer, glycidyl methacrylate, component three, and dicumyl peroxide is 10g: 0.1-0.5g: 8-12g: 0.4-0.6g.

6. A method for preparing moisture-proof and antibacterial bamboo charcoal bristles according to claim 1, It is characterized in that The process parameters of the twin-screw extruder in S1 are set as follows: zone 1 200-210℃, zone 2 210-220℃, zone 3 230-235℃, zone 4 240-250℃, zone 5 250-260℃, and the speed of the twin-screw extruder is 160-180rpm; the process parameters of the twin-screw extruder in A4 are set as follows: zone 1 160-170℃, zone 2 160-170℃, zone 3 160-170℃, zone 4 170-180℃, zone 5 170-180℃, zone 6 170-180℃, zone 7 170-180℃, and the screw speed is 50-60rpm.

7. The method for preparing moisture-proof and antibacterial bamboo charcoal bristles according to claim 1, It is characterized in that The process parameters of the melt spinning machine were set as follows: temperature 230-240°C, draft ratio 4.80-4.

95.

8. A moisture-proof and antibacterial bamboo charcoal brush bristle, It is characterized in that The invention is made by the preparation method of moisture-proof and antibacterial bamboo charcoal bristles described in any one of claims 1 to 7.

9. Use of the moisture-proof and antibacterial bamboo charcoal bristles as claimed in claim 8 in a toothbrush.