A device system and method for continuous production of precious metal-loaded catalysts
Through the immersion-precipitation reaction and redox reaction in the continuous production device system, combined with atomization and calcination steps, the problems of complex preparation process and low production capacity of precious metal-supported catalysts are solved, and the high production capacity and excellent dispersion of active components are achieved. Effect.
Patent Information
- Application Number
- CN202411067387.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing precious metal-supported catalysts have complex preparation processes, large investment, low production capacity, and difficult to achieve high loading rate and good dispersion of active components.
The continuous production device system is adopted, including the first tube reaction device, the second tube reaction device, the atomization device and the roasting device. Through the impregnation-precipitation reaction, the redox reaction, the atomization and the roasting device, the multi-layer cross-arrangement is used The mixing unit sheet and distribution device realize the full mixing of materials and the regulation of catalyst particle size.
It realizes continuous production of precious metal-supported catalysts with high productivity and good dispersion of active components, simplifies the process flow, reduces the wear rate of the catalyst, and is suitable for industrial production.
Smart Images

Figure CN118577226B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and relates to a device system and method for continuously producing precious metal-loaded catalysts. Background Art
[0002] Supported metal catalysts are widely used in hydrogenation reactions. To obtain better structural stability, noble metals are usually supported on a carrier before being used in hydrogenation reactions. The existing preparation methods of supported metal catalysts mainly include coprecipitation and impregnation.
[0003] The co-precipitation method is to evenly mix the carrier and the metal precursor and add a precipitant to precipitate, followed by a series of steps such as filtration, washing, drying, roasting, activation, etc. The catalyst prepared by this method has the advantages of uniform dispersion of active components, easy control of catalyst specific surface, pore volume, and pore size, and is often used in the preparation of supported transition metal catalysts such as Fe, Co, Ni, and Cu. However, when this method is used in the preparation of precious metal supported catalysts, there are often problems such as metal sintering and strong interaction between the metal and the carrier during the roasting process, resulting in low catalyst activity. Therefore, it is not commonly used in industry.
[0004] Supported precious metal catalysts are usually prepared in industry by the impregnation method, which is divided into dry impregnation and wet impregnation. Among them, dry impregnation is often used to prepare spherical, columnar and other shaped supported catalysts to obtain "eggshell" or "protein" catalysts with lower loading rates, while its use in the preparation of powdered precious metal catalysts has problems such as uneven distribution of active components and difficulty in achieving high loading rates. Wet impregnation uses an excess of active metal precursor solution, so the metal dispersion effect is better during the impregnation process, but metal ion migration is prone to occur during the drying process, resulting in uneven secondary distribution, and the final catalyst activity is also low.
[0005] At present, the preparation process of precious metal-loaded catalysts is generally complicated, and most of them are intermittent operations, which have the problems of large investment and low production capacity; in addition, there are few research reports on the optimization of corresponding equipment.
[0006] In summary, there is an urgent need to provide a device system and method for producing precious metal-loaded catalysts with simple process, high production capacity, continuous production and excellent catalyst performance. Summary of the invention
[0007] The object of the present invention is to provide a device system and method for continuously producing precious metal-loaded catalysts, which can realize the continuous production of precious metal-loaded catalysts and greatly improve the production capacity. The active components of the obtained catalysts have good dispersibility and stable activity.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a device system for continuously producing a noble metal-supported catalyst, wherein along the direction of material flow, the device system comprises a first tubular reaction device, a second tubular reaction device, an atomizing device, a drying device, and a calcining device which are sequentially connected;
[0010] The first tubular reaction device is independently provided with a first feed inlet, a second feed inlet and a third feed inlet;
[0011] The first tubular reaction device is provided with a plurality of layers of mixing unit sheets;
[0012] The hybrid unit sheets are arranged in a left-right cross pattern;
[0013] The second tubular reaction device is independently provided with a fourth feed inlet and a fifth feed inlet;
[0014] The second tubular reaction device is provided with a distribution device.
[0015] The device system provided by the present invention is provided with a first tubular reaction device, a second tubular reaction device, an atomizing device, a drying device and a calcining device in sequence along the direction of material flow, which can realize the continuous production of precious metal-loaded catalysts and greatly improve the production capacity. At the same time, the equipment of the device system is simple and flexible, and can meet the needs of later process adjustments.
[0016] It is worth noting that the present invention has several layers of mixing unit sheets arranged in a left-right cross pattern in the first tubular reaction device, and a distribution device is arranged in the second tubular reaction device, which can not only achieve sufficient mixing of materials, but also effectively control the catalyst particle size.
[0017] As a preferred technical solution of the present invention, the first tubular reaction device includes a serpentine tubular reaction device.
[0018] The first feed inlet and the second feed inlet are independently arranged on the side wall of the first tubular reaction device.
[0019] The third feed inlet is arranged at the top of the first tubular reaction device.
[0020] As a preferred technical solution of the present invention, the mixing unit sheet is arranged at the lower part of the first feed port, the second feed port and the third feed port.
[0021] In the present invention, a high-pressure feed pump and a feed pipeline are independently arranged between the first feed port, the second feed port and the third feed port and their respective raw materials.
[0022] In the present invention, the number of layers of the hybrid unit sheet is set according to the required production load and after determining the tube diameter and tube length of the first tubular reaction device. Those skilled in the art can set the number of layers according to actual needs.
[0023] The maximum rotation angle of the hybrid unit sheet between left and right rotation is 45-60°, for example, it can be 47°, 50°, 52°, 55°, 56° or 58°, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] The maximum spacing between the left and right rotations of the hybrid unit sheet is 5-10 mm, for example, it can be 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 9 mm or 9.5 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] In the present invention, the maximum distance between the left and right rotations of the hybrid unit sheet is the maximum distance between the left and right rotations at the wall surface of the hybrid unit sheet.
[0026] It is worth noting that the present invention further improves the mixing degree of the materials by controlling the maximum rotation angle and the maximum spacing range between the left and right rotation of the mixing unit sheet, so that the materials can fully undergo an impregnation-precipitation reaction in the first tubular reaction device.
[0027] As a preferred technical solution of the present invention, the discharge port of the first tubular reaction device is communicated with the feed port of the second tubular reaction device.
[0028] The second tubular reaction device comprises a multi-pass tubular reaction device.
[0029] The second tubular reaction device is provided with a heat-insulating jacket outside.
[0030] In the present invention, the material of the first tubular reaction device, the second tubular reaction device and the pipeline includes any one of non-metal, 304 stainless steel or 316L stainless steel.
[0031] The second tubular reaction device is provided with a plurality of reaction tubes with top openings; the plurality of reaction tubes are arranged in parallel.
[0032] In the present invention, the number of the reaction tubes is greater than 20.
[0033] The fourth feed inlet and the fifth feed inlet are independently arranged on the side wall of the second tubular reaction device.
[0034] The distribution device is arranged at the upper part of the reaction tube and is communicated with the pipeline of the fifth feed inlet.
[0035] The distribution device is provided with distribution holes, and the distribution holes are arranged in one-to-one correspondence with the reaction tubes.
[0036] As a preferred technical solution of the present invention, the discharge port of the second tubular reaction device is connected to the atomization device.
[0037] The atomizing device is provided with a shearing disk and an atomizing nozzle.
[0038] In the present invention, there is no specific limitation on the number of shear discs and atomizing nozzles, and those skilled in the art may select and set them according to actual production needs.
[0039] The atomizing nozzle is provided with a plurality of discharge holes.
[0040] In the present invention, the discharge holes are evenly distributed on the atomizing nozzle.
[0041] The diameter of the discharge hole is 50-100 μm, for example, it can be 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm or 95 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] The atomizing device is arranged in the drying device.
[0043] In the present invention, the drying device comprises a drying tower.
[0044] An exhaust port is arranged on the top of the drying device.
[0045] The material outlet of the drying device is communicated with the roasting device.
[0046] In the present invention, the roasting device comprises a rotary kiln.
[0047] In a second aspect, the present invention provides a method for continuously producing a noble metal supported catalyst, the method being carried out using the device system described in the first aspect, comprising the following steps:
[0048] (1) respectively feeding a precious metal salt solution through a first feed port, a precipitant solution through a second feed port, and a carrier slurry through a third feed port, then mixing the mixture through a mixing unit sheet, and performing an impregnation-precipitation reaction in a first tubular reaction device to obtain a first material;
[0049] (2) Step (1) The first material is introduced into a second tubular reaction device, a reducing agent solution is fed into the second tubular reaction device through the fourth feed port, and steam is fed into the second feed port, and an oxidation-reduction reaction is carried out in the second tubular reaction device to obtain a second material;
[0050] (3) Step (2) The second material is atomized by an atomizing device, dried by a drying device, and calcined by a calcining device to obtain the precious metal-supported catalyst.
[0051] The method provided by the present invention can prepare a noble metal-supported catalyst with good active component dispersibility and stable activity through sequential impregnation-precipitation reaction, oxidation-reduction reaction, atomization, drying and calcination. The method is simple in process, easy to operate and suitable for industrial production.
[0052] It is worth noting that the present invention adopts the impregnation-precipitation method to mix the raw materials, combining the advantages of wet impregnation and co-precipitation methods, that is, firstly, an excess of precious metal precursor solution is fully mixed with the carrier slurry to make the metal precursor highly dispersed in the carrier pores, and then a reducing agent is introduced for oxidation-reduction, and the precipitant is used to convert the metal precursor into a precipitate to anchor it in the carrier channel, so that no secondary migration of the metal will occur in the subsequent drying and calcination steps.
[0053] As a preferred technical solution of the present invention, the feed molar ratio of the precious metal in the precious metal salt solution in step (1) to the precipitant in the precipitant solution is 1:(7-12), for example, it can be 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:10.5, 1:11 or 1:11.5, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0054] The feed molar ratio of the precious metal in the precious metal salt solution in step (1) to the carrier in the carrier slurry is 1:(30-80), for example, it can be 1:35, 1:40, 1:45, 1:50, 1:55, 1:60, 1:65, 1:70 or 1:75, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0055] The mass concentration of the noble metal salt solution in step (1) is 8-12wt%, for example, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt%, 11wt% or 11.5wt%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0056] The noble metal salt solution in step (1) includes any one of a ruthenium salt solution, a rhodium salt solution or a palladium salt solution, or a combination of at least two of them.
[0057] The mass concentration of the precipitant solution in step (1) is 8-15wt%, for example, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt%, 11wt%, 11.5wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt% or 14.5wt%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0058] The precipitant solution in step (1) comprises a sodium hydroxide solution.
[0059] The mass concentration of the carrier slurry in step (1) is 8-15wt%, for example, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt%, 11wt%, 11.5wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt% or 14.5wt%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0060] The carrier slurry in step (1) includes any one of alumina slurry, zirconium oxide slurry, activated carbon slurry, silicon oxide slurry or molecular sieve slurry.
[0061] In step (1), the material needs to be preheated before feeding, and the preheating temperature is 55-65°C, for example, it can be 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C or 64°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0062] In the present invention, the inlet temperature and outlet temperature of the material in the first tubular reaction device are the same, and there is no temperature gradient.
[0063] As a preferred technical solution of the present invention, the pressure of the first tubular reaction device in step (1) is 10000-15000 KpaA, for example, it can be 10500 KpaA, 11000 KpaA, 11500 KpaA, 12000 KpaA, 13000 KpaA, 14000 KpaA or 14500 KpaA, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0064] The residence time of the material in the first tubular reaction device in step (1) is 30-60 min, for example, 32 min, 35 min, 38 min, 40 min, 42 min, 45 min, 48 min, 50 min, 52 min, 55 min or 58 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0065] The flow rate of the material in the first tubular reaction device in step (1) is 0.5-1.5 m / s, for example, 0.6 m / s, 0.7 m / s, 0.8 m / s, 0.9 m / s, 1 m / s, 1.1 m / s, 1.2 m / s, 1.3 m / s or 1.4 m / s, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0066] In the present invention, the diameter and length of the first tubular reaction device are adjusted according to the residence time and flow rate of the material in the first tubular reaction device.
[0067] As a preferred technical solution of the present invention, the feed molar ratio of the reducing agent in the reducing agent solution of step (2) to the precious metal in the precious metal salt solution is 1:(0.08-0.12), for example, it can be 1:0.085, 1:0.09, 1:0.095, 1:0.1, 1:0.105, 1:0.11 or 1:0.115, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0068] The mass concentration of the reducing agent solution in step (2) is 8-12wt%, for example, 8.5wt%, 9wt%, 9.5wt%, 10wt%, 10.5wt%, 11wt% or 11.5wt%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0069] The reducing agent in the reducing agent solution in step (2) includes sodium formate.
[0070] The temperature of the second tubular reaction apparatus in step (2) is 75-85°C, for example, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C or 84°C, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0071] In the present invention, hot steam is introduced to heat the second tubular reaction device, and the amount of heating medium matches the heat load, so that the temperature of the second tubular reaction device is 75-85°C.
[0072] The pressure of the second tubular reaction apparatus in step (2) is 10000-12000 KpaA, for example, 10200 KpaA, 10500 KpaA, 10800 KpaA, 11000 KpaA, 11200 KpaA, 11500 KpaA or 11800 KpaA, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0073] The residence time of the material in the second tubular reaction device in step (2) is 10-40 min, for example, it can be 12 min, 15 min, 18 min, 20 min, 22 min, 25 min, 28 min, 30 min, 32 min, 35 min or 38 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0074] The flow rate of the material in the second tubular reaction device in step (2) is 0.6-1.0 m / s, for example, 0.65 m / s, 0.7 m / s, 0.75 m / s, 0.8 m / s, 0.85 m / s, 0.9 m / s or 0.95 m / s, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0075] As a preferred technical solution of the present invention, the rotation speed of the shear disk in the atomization device in step (3) is 12000-15000 r / min, for example, it can be 12500 r / min, 13000 r / min, 13500 r / min, 14000 r / min or 14500 r / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0076] The pressure of the drying device in step (3) is -1KpaG~1KpaG, and the temperature is 100-200°C.
[0077] In the present invention, the pressure in the drying device is a slight negative pressure; the temperature of the drying device is 100-200°C, for example, it can be 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0078] The atmosphere in the roasting device in step (3) is an inert atmosphere.
[0079] In the present invention, the inert atmosphere includes nitrogen.
[0080] The pressure of the roasting device in step (3) is -1KpaG~1KpaG, the temperature is 400-600°C, and the residence time is 4-6h.
[0081] In the present invention, the roasting device is continuously operated, and its pressure is a slightly positive pressure. The temperature of the roasting device is 400-600°C, for example, it can be 420°C, 450°C, 480°C, 500°C, 520°C, 540°C, 550°C or 580°C, etc. The residence time of the roasting device is 4-6h, for example, it can be 4.2h, 4.5h, 4.8h, 5h, 5.2h, 5.5h or 5.8h, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0082] The wear rate of the noble metal supported catalyst is ≤2%, for example, it can be 1.8%, 1.6%, 1.5%, 1.2%, 1%, 0.8% or 0.5%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably ≤1.5%.
[0083] In the present invention, the D50 particle size of the obtained noble metal supported catalyst is 25-35 μm. The method provided by the present invention can not only effectively control the catalyst particle size, but also greatly reduce the catalyst wear rate.
[0084] Compared with the prior art, the present invention has the following beneficial effects:
[0085] (1) The device system provided by the present invention can realize the continuous production of precious metal-loaded catalysts, and the production capacity is greatly improved. At the same time, the equipment of the device system is simple and flexible, and can meet the needs of later process adjustment. Furthermore, by providing a plurality of layers of mixing unit sheets in the first tubular reaction device, and the mixing unit sheets are arranged in a left-right cross pattern, and providing a distribution device in the second tubular reaction device, not only can the materials be fully mixed, but also the catalyst particle size can be effectively regulated.
[0086] (2) The method provided by the present invention can produce a precious metal-supported catalyst with good active component dispersion and stable activity after sequentially undergoing impregnation-precipitation reaction, oxidation-reduction reaction, atomization, drying and calcination; the method is simple in process, easy to operate and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0087] Figure 1 A schematic diagram of the device system for continuously producing precious metal-supported catalysts provided in Example 1;
[0088] Figure 2 Schematic diagram of part of the first tubular reaction device and part of the second tubular reaction device provided in Example 1, α is the maximum rotation angle between left and right rotation of the mixing unit sheet;
[0089] Among them, 1-first feed port, 2-second feed port, 3-third feed port, 4-first tubular reaction device, 5-fourth feed port, 6-fifth feed port, 7-second tubular reaction device, 8-atomization device, 9-drying device, 10-exhaust port, 11-rotary kiln, 12-mixing unit sheet, 13-distribution device. DETAILED DESCRIPTION
[0090] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0091] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0092] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0093] In the following embodiments and comparative examples, the number of layers of the hybrid unit sheet is adjusted according to the required production load, and those skilled in the art can make the selection according to the actual situation.
[0094] Example 1
[0095] This embodiment provides a device system for continuously producing a noble metal supported catalyst (such as Figure 1-2 As shown), along the direction of material flow, the device system includes a first tubular reaction device 4, a second tubular reaction device 7, an atomizing device 8, a drying device 9 and a rotary kiln 11 which are connected in sequence;
[0096] The side wall of the first tubular reaction device 4 is independently provided with a first feed inlet 1 and a second feed inlet 2; the top of the first tubular reaction device 4 is provided with a third feed inlet 3;
[0097] The first tubular reaction device 4 is a serpentine tubular reaction device; a plurality of layers of mixing unit sheets 12 are arranged in the first tubular reaction device 4; the mixing unit sheets 12 are arranged at the lower part of the first feed port 1, the second feed port 2 and the third feed port 3; the mixing unit sheets 12 are arranged crosswise in left-right rotation; the maximum rotation angle of the mixing unit sheets 12 between left-right rotation is 50° and the maximum spacing is 8mm;
[0098] The discharge port of the first tubular reaction device 4 is connected to the feed port of the second tubular reaction device 7; the side walls of the second tubular reaction device 7 are independently provided with a fourth feed port 5 and a fifth feed port 6;
[0099] The second tubular reaction device 7 is provided with a heat-insulating jacket outside; 150 reaction tubes with top openings are provided inside the second tubular reaction device 7; the reaction tubes are arranged in parallel; a distribution device 13 is provided inside the second tubular reaction device 7; the distribution device 13 is arranged at the upper part of the reaction tube and is connected with the pipeline of the fifth feed port 6; the distribution device 13 is provided with distribution holes, and the distribution holes are arranged one by one with the reaction tubes;
[0100] The discharge port of the second tubular reaction device 7 is connected to the atomizing device 8; the atomizing device 8 is provided with a shearing disk and 50 atomizing nozzles; the atomizing nozzles are provided with 50 discharge holes (and the discharge holes discharge into the same atomizing shearing disk); the atomizing device 8 is provided in the drying device 9; the top of the drying device 9 is provided with an exhaust port 10; the discharge port of the drying device 9 is connected to the rotary kiln 11.
[0101] Example 2
[0102] This embodiment provides a device system for continuously producing a noble metal supported catalyst, which further defines the following on the basis of the device system provided in Example 1:
[0103] The first tubular reaction device, the second tubular reaction device and the pipeline are all made of 306L stainless steel; the diameter of the discharge hole is 80 μm.
[0104] Example 3
[0105] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum rotation angle between left and right rotation of the mixing unit sheet is 40° and the maximum spacing is 10 mm, other conditions are the same as those in Embodiment 1.
[0106] Example 4
[0107] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum rotation angle between left and right rotation of the mixing unit sheet is 60° and the maximum spacing is 5 mm, other conditions are the same as those in Embodiment 1.
[0108] Example 5
[0109] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum rotation angle between left and right rotation of the mixing unit sheet is 30°, other conditions are the same as those in Embodiment 1.
[0110] Example 6
[0111] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum rotation angle between left and right rotation of the mixing unit sheet is 75°, other conditions are the same as those in Embodiment 1.
[0112] Example 7
[0113] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum spacing between the left and right rotations of the mixing unit sheet is 3 mm, other conditions are the same as those in Embodiment 1.
[0114] Example 8
[0115] This embodiment provides a device system for continuously producing precious metal-loaded catalysts. Except that the maximum spacing between the left and right rotations of the mixing unit sheet is 15 mm, other conditions are the same as those in Embodiment 1.
[0116] Comparative Example 1
[0117] This comparative example provides a device system for continuously producing a precious metal-loaded catalyst. Except that the first tubular reaction device is not provided with a second feed inlet, other conditions are the same as those of Example 1.
[0118] Comparative Example 2
[0119] This comparative example provides a device system for continuously producing precious metal-supported catalysts. Except that no mixing unit sheet is provided in the first tubular reaction device, other conditions are the same as those in Example 1.
[0120] Comparative Example 3
[0121] This comparative example provides a device system for continuously producing precious metal-loaded catalysts. Except that no distribution device is provided in the second tubular reaction device, other conditions are the same as those in Example 1.
[0122] Application Example 1
[0123] This application example provides a method for continuously producing a noble metal supported catalyst, the method being carried out using the device system provided in Example 1, comprising the following steps:
[0124] (1) simultaneously feeding a ruthenium chloride solution having a temperature of 60° C. and 10 wt% through a first feed port at a rate of 30 kg / h, feeding a sodium hydroxide solution having a temperature of 60° C. and 10 wt% through a second feed port at a rate of 57.8 kg / h, and feeding an alumina slurry having a temperature of 60° C. and 10 wt% through a third feed port at a rate of 832.6 kg / h, and then mixing the mixture through a mixing unit sheet, and performing an impregnation-precipitation reaction in a first tubular reaction device to obtain a first material;
[0125] The pressure of the first tubular reaction device is 10000 KpaA; the material residence time is 60 min, and the material flow rate is 0.8 m / s; the outlet temperature of the first tubular reaction device is 60° C.;
[0126] (2) Step (1) The first material is introduced into a second tubular reaction device, and at the same time, a 10 wt% sodium formate solution is fed through the fourth feed port at a rate of 103 kg / h, and hot steam is fed through the fifth feed port, and a redox reaction is carried out in the second tubular reaction device to obtain a second material;
[0127] The temperature of the second tubular reaction device is 80°C and the pressure is 10000KpaA; the material residence time is 40min and the material flow rate is 1.0m / s;
[0128] (3) The second material in step (2) is atomized by an atomizing device, dried by a drying device and calcined in a rotary kiln to obtain the noble metal-supported catalyst;
[0129] The rotation speed of the shear disk in the atomization device is 11000 rpm;
[0130] The pressure of the drying device is -0.5 kpaG and the temperature is 200°C;
[0131] The atmosphere of the rotary kiln is nitrogen, the pressure is 0.5 kpaG, the temperature is 500° C., and the residence time is 4 hours.
[0132] Application Example 2
[0133] This application example provides a method for continuously producing a precious metal-loaded catalyst, which is carried out using the device system provided in Example 2, except that a rhodium chloride solution with a temperature of 60°C and 10wt% is fed through the first feed port at a rate of 30kg / h, a sodium hydroxide solution with a temperature of 60°C and 10wt% is fed through the second feed port at a rate of 44kg / h, an alumina slurry with a temperature of 60°C and 10wt% is fed through the third feed port at a rate of 921kg / h, and the rotation speed of the shear disk in the atomizing device is 12000rpm; other conditions are the same as those in Application Example 1.
[0134] Application Example 3
[0135] This application example provides a method for continuously producing precious metal-loaded catalysts, which is carried out using the device system provided in Example 3, except that the feed rate of the silicon oxide slurry is adjusted to 628.5 kg / h, the temperature of the second tubular reactor is 75°C, and the residence time in the rotary kiln is 5 hours; other conditions are the same as those in Application Example 1.
[0136] Application Example 4
[0137] This application example provides a method for continuously producing precious metal loaded catalysts, which is carried out using the device system provided in Example 4, except that the feed rate of the zirconium oxide slurry is adjusted to 615.3 kg / h, the temperature of the second tubular reactor is 85°C, the rotation speed of the shear disk in the atomizing device is 14000 rpm, and the temperature of the rotary kiln is 550°C; other conditions are the same as those in Application Example 1.
[0138] Application Example 5
[0139] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 5, and other conditions are the same as those in Application Example 1.
[0140] Application Example 6
[0141] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 6, and other conditions are the same as those in Application Example 1.
[0142] Application Example 7
[0143] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 7, and other conditions are the same as those in Application Example 1.
[0144] Application Example 8
[0145] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 8, and other conditions are the same as those in Application Example 1.
[0146] Application Example 9
[0147] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 1. Except that the residence time of the material in the first tubular reaction device is 10 minutes, other conditions are the same as those in Application Example 1.
[0148] Application Example 10
[0149] This application example provides a method for continuously producing precious metal-loaded catalysts. The method is carried out using the device system provided in Example 1. Except that the residence time of the material in the first tubular reaction device is 80 minutes, other conditions are the same as those in Application Example 1.
[0150] Comparative application example 1
[0151] This comparative application example provides a method for continuously producing a precious metal-loaded catalyst. The method is carried out using the device system provided in Comparative Example 1, and other conditions are the same as those in Application Example 1.
[0152] Comparative Application Example 2
[0153] This comparative application example provides a method for continuously producing a precious metal-loaded catalyst. The method is carried out using the device system provided in Comparative Example 2, and other conditions are the same as those in Application Example 1.
[0154] Comparative Application Example 3
[0155] This comparative application example provides a method for continuously producing a precious metal-loaded catalyst. The method is carried out using the device system provided in Comparative Example 3, and other conditions are the same as those in Application Example 1.
[0156] The particle size distribution, wear rate and yield of the catalysts prepared in the above application examples and comparative application examples were tested, wherein the particle size distribution was tested using a laser particle size analyzer, and the wear rate was tested using a HT9801 FCC catalyst wear index tester; the results are shown in Table 1.
[0157] Table 1
[0158]
[0159] Wherein, “ / ” indicates that no catalyst product was obtained;
[0160] From Table 1, we can see that:
[0161] (1) The device system and method provided by the present invention can realize the continuous production of precious metal-loaded catalysts, greatly improve production capacity, and can adjust the D50 particle size distribution of the catalyst. At the same time, the wear rate is low, less than 1.5%. In addition, the device system provided by the present invention is highly flexible and can be realized for catalyst modification requirements in different scenarios;
[0162] (2) By comparing Application Example 1 with Application Examples 5-8, it can be seen that when the maximum rotation angle between the left and right rotations of the unit sheet is too small or the maximum spacing between the left and right rotations of the unit sheet is too small, the manufacturing is difficult and the flow pressure drop increases, the corresponding manufacturing cost increases and a higher conveying pressure is required, which leads to a slight increase in the wear rate; when the maximum rotation angle between the left and right rotations of the unit sheet is too large or the maximum spacing between the left and right rotations of the unit sheet is too large, the turbulence effect is insufficient, resulting in uneven material mixing, which in turn affects the distribution of active components and the D50 particle size distribution of the catalyst;
[0163] (3) From the comparison between Application Example 1 and Application Examples 9-10, it can be seen that when the time of the impregnation-precipitation reaction is too short, due to the incomplete impregnation-precipitation reaction, some active substances may not be fully mixed with the carrier; when the time of the impregnation-precipitation reaction is too long, it has no obvious effect on the reaction itself, but it will increase the design length of the tubular reactor, resulting in a waste of production costs;
[0164] (4) From the comparison between Comprehensive Application Example 1 and Comparative Application Example 1, it can be seen that when the first tubular reaction device is not provided with the second feed port, the material in the first tubular reaction device is only subjected to an impregnation reaction, and metal ion migration is likely to occur during the drying process, and the desired catalyst product cannot be obtained;
[0165] (5) From the comparison between Application Example 1 and Comparative Application Examples 2-3, it can be seen that when the first tubular reaction device is not provided with a mixing unit sheet or the second tubular reaction device is not provided with a distribution device, it is not conducive to the full mixing of the materials, resulting in a decrease in the yield of the catalyst and the inability to effectively control the catalyst particle size.
[0166] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for continuously producing a noble metal supported catalyst, It is characterized in that The method is carried out using the following device system: Along the direction of material flow, the device system includes a first tubular reaction device, a second tubular reaction device, an atomizing device, a drying device and a roasting device which are connected in sequence; The first tubular reaction device is independently provided with a first feed inlet, a second feed inlet and a third feed inlet; a plurality of layers of mixing unit sheets are arranged in a left-right rotation cross pattern in the first tubular reaction device; The second tubular reaction device is independently provided with a fourth feed inlet and a fifth feed inlet; a distribution device is provided in the second tubular reaction device; the distribution device is provided at the upper part of the reaction tube and is connected with the pipeline of the fifth feed inlet; a plurality of reaction tubes with top openings are provided in the second tubular reaction device; the plurality of reaction tubes are arranged in parallel; The method comprises the following steps: (1) respectively feeding a precious metal salt solution through a first feed port, a precipitant solution through a second feed port, and a carrier slurry through a third feed port, then mixing the mixture through a mixing unit sheet, and performing an impregnation-precipitation reaction in a first tubular reaction device to obtain a first material; (2) Step (1) The first material is introduced into a second tubular reaction device, a reducing agent solution is fed into the second tubular reaction device through the fourth feed port, and steam is fed into the second feed port, and an oxidation-reduction reaction is carried out in the second tubular reaction device to obtain a second material; (3) Step (2) The second material is atomized by an atomizing device, dried by a drying device, and calcined by a calcining device to obtain the precious metal-supported catalyst.
2. The method according to claim 1, It is characterized in that The first tubular reaction device comprises a serpentine tubular reaction device; The first feed inlet and the second feed inlet are independently arranged on the side wall of the first tubular reaction device; The third feed inlet is arranged at the top of the first tubular reaction device.
3. The method according to claim 1, It is characterized in that The mixing unit sheet is arranged at the lower part of the first feed port, the second feed port and the third feed port; The maximum rotation angle between left and right rotation of the hybrid unit sheet is 45-60°; The maximum spacing between the left and right rotations of the hybrid unit sheet is 5-10 mm.
4. The method according to claim 1, It is characterized in that The discharge port of the first tubular reaction device is connected to the feed port of the second tubular reaction device; The second tubular reaction device comprises a multi-pass tubular reaction device; The second tubular reaction device is provided with a heat-insulating jacket outside; The fourth feed inlet and the fifth feed inlet are independently arranged on the side wall of the second tubular reaction device; The distribution device is provided with distribution holes, and the distribution holes are arranged in one-to-one correspondence with the reaction tubes.
5. The method according to claim 1, It is characterized in that The discharge port of the second tubular reaction device is connected to the atomization device; The atomizing device is provided with a shearing disk and an atomizing nozzle; The atomizing nozzle is provided with a plurality of discharge holes; The diameter of the discharge hole is 50-100 μm; The atomizing device is arranged in the drying device; An exhaust port is provided on the top of the drying device; The material outlet of the drying device is communicated with the roasting device.
6. The method according to claim 1, It is characterized in that The feed molar ratio of the noble metal in the noble metal salt solution to the precipitant in the precipitant solution in step (1) is 1:(7-12); The feed molar ratio of the noble metal in the noble metal salt solution to the carrier in the carrier slurry in step (1) is 1:(30-80); The mass concentration of the noble metal salt solution in step (1) is 8-12wt%; The noble metal salt solution in step (1) includes any one of a ruthenium salt solution, a rhodium salt solution or a palladium salt solution, or a combination of at least two thereof; The mass concentration of the precipitant solution in step (1) is 8-15wt%; The precipitant solution in step (1) comprises a sodium hydroxide solution; The mass concentration of the carrier slurry in step (1) is 8-15wt%; The carrier slurry in step (1) includes any one of alumina slurry, zirconium oxide slurry, activated carbon slurry, silicon oxide slurry or molecular sieve slurry; In step (1), the material needs to be preheated before feeding, and the preheating temperature is 55-65°C.
7. The method according to claim 1, It is characterized in that Step (1) The pressure of the first tubular reaction device is 10000-15000 KPaA; The residence time of the material in the first tubular reaction device in step (1) is 30-60 minutes; The flow rate of the material in the first tubular reaction device in step (1) is 0.5-1.5 m / s.
8. The method according to claim 1, It is characterized in that In step (2), the feed molar ratio of the reducing agent in the reducing agent solution to the precious metal in the precious metal salt solution is 1:(0.08-0.12); The mass concentration of the reducing agent solution in step (2) is 8-12wt%; The reducing agent in the reducing agent solution of step (2) comprises sodium formate; Step (2) The temperature of the second tubular reaction device is 75-85°C; Step (2) The pressure of the second tubular reaction device is 10000-12000 KPaA; The residence time of the material in the second tubular reaction device in step (2) is 10-40 minutes; The flow rate of the material in the second tubular reaction device in step (2) is 0.6-1.0 m / s.
9. The method according to claim 1, It is characterized in that The rotation speed of the shear disk in the atomizing device in step (3) is 12000-15000 r / min; The pressure of the drying device in step (3) is -1kpaG~1kpaG, and the temperature is 100-200°C; The atmosphere in the roasting device in step (3) is an inert atmosphere; Step (3) The pressure of the roasting device is -1kpaG~1kpaG, the temperature is 400-600°C, and the residence time is 4-6h; The wear rate of the noble metal supported catalyst is ≤2%.
Citation Information
Patent Citations
Bimetal supported molecular sieve catalyst as well as preparation method and application thereof
CN114950542A
System and method for continuously producing low-valence chromium-loaded catalyst
CN115779977A
Spinning polyester fuse -element static mixer
CN208414647U
Hydrodealkylation of alkylaromatic hydrocarbons
US4138443A