Lignite-based honeycomb activated carbon and preparation method thereof

By acidizing and heat treatment of lignite powder, combined with isopropyl titanate precursor solution and rosin-based quaternary ammonium salt, the problem of lignite-based honeycomb activated carbon is solved, and high mechanical strength, good hydrophobicity and adsorption are obtained. Honeycomb activated carbon with good effect.

CN118579781BActive Publication Date: 2024-11-08HANGZHOU HUISHUI TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411046610.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-08
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Lignite-based honeycomb activated carbon is prone to cracking, whitening, and has poor adsorption effect. The prior art requires the addition of a large amount of adhesive to enhance mechanical strength, but it leads to a decrease in carbon content and a decrease in adsorption effect.

Method used

By acidizing the lignite powder and adding isopropyl titanate precursor solution and rosin-based quaternary ammonium salt, plastic coal sludge is formed, and heat treatment is carried out after extrusion and molding to produce lignite-based honeycomb activated carbon that is not easy to turn white and has high mechanical strength.

Benefits of technology

The mechanical strength improvement, hydrophobicity enhancement and adsorption effect of lignite-based honeycomb activated carbon has been achieved, and it is especially suitable for adsorbing volatile organic matter in gases with high humidity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a lignite-based honeycomb activated carbon and a preparation method thereof, wherein the preparation method of the lignite-based honeycomb activated carbon comprises the following steps: taking lignite powder, acidifying to obtain acidified coal powder; adding an organic binder and water to the acidified coal powder, mixing evenly, adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading, and mixing evenly to obtain plastic coal slime; loading the plastic coal slime into an extrusion molding machine, extruding a honeycomb blank; heat-treating the honeycomb blank to obtain lignite-based honeycomb activated carbon. The lignite-based honeycomb activated carbon obtained by the preparation method of the present invention is not easy to turn white, is not easy to crack, has good mechanical strength, and has good hydrophobicity and adsorption effect, and is particularly suitable for adsorbing volatile organic matter in gases with high humidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of activated carbon preparation, in particular to a lignite-based honeycomb activated carbon and a preparation method thereof. Background Art

[0002] Lignite, also known as wood coal, is a brown-black, dull, low-grade coal between peat and bituminous coal. Lignite has the characteristics of high moisture and high volatile components, poor thermal stability, strong chemical reactivity, easy weathering in the air, difficult to store and transport over long distances, and serious air pollution when burned. Therefore, the deep processing and comprehensive utilization of lignite are of great significance.

[0003] Since lignite has low carbon content, many impurities, poor mechanical strength and is easy to break, using lignite as raw material for preparing honeycomb activated carbon is prone to problems such as cracking and whitening of finished products. In order to improve the mechanical properties of honeycomb activated carbon, the existing technology often needs to add a large amount of adhesive to enhance the mechanical strength of honeycomb activated carbon. However, this will further reduce the carbon content of lignite-based honeycomb activated carbon and reduce the adsorption effect. Summary of the invention

[0004] The purpose of the present invention is to provide a lignite-based honeycomb activated carbon to solve the problems of easy cracking, whitening and poor adsorption effect of lignite-based honeycomb activated carbon in the prior art.

[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows:

[0006] A method for preparing lignite-based honeycomb activated carbon comprises the following steps:

[0007] (1) taking lignite powder and acidifying it to obtain acidified coal powder;

[0008] (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained;

[0009] (3) loading the plastic coal slime in step (2) into an extruder to extrude and form a honeycomb blank;

[0010] (4) The honeycomb blank in step (3) is heat-treated to obtain lignite-based honeycomb activated carbon.

[0011] Preferably, in step (1), the acidification specifically comprises: immersing the lignite powder in an acid solution, stirring at 20-50° C. for 1-3 hours, and filtering;

[0012] The acid solution is one of hydrochloric acid and nitric acid; the concentration of the acid solution is 4-6 mol / L.

[0013] Preferably, step (1) further includes the step of crushing the lignite powder to a particle size less than or equal to 2 mm.

[0014] Preferably, in step (2), the isopropyl titanate precursor solution is prepared by mixing isopropyl titanate and water in a volume ratio of 1:(80-100).

[0015] Preferably, in step (2), the weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:(2-6):(3-5):(5-8):(0.1-0.8).

[0016] Preferably, the rosin-based quaternary ammonium salt has a structure as shown in formula (I):

[0017]

[0018] (I)

[0019] Wherein, R has a structure as shown in formula (II):

[0020]

[0021] (II)

[0022] Preferably, the rosin-based quaternary ammonium salt has a structure as shown in formula (III):

[0023]

[0024] (III)

[0025] Preferably, in step (2), the organic binder is one or more of urea-formaldehyde resin, hydroxyethyl cellulose, polyvinyl alcohol, and sodium carboxymethyl cellulose.

[0026] Preferably, in step (3), the extrusion molding pressure is 12-15 MPa.

[0027] Preferably, the heat treatment in step (4) comprises: first maintaining at 100-150°C for 1-2 hours, then heating to 300-500°C at a rate of 2-6°C / min under the protection of an inert gas, and maintaining for 1-2 hours; then, carbonizing at 600-700°C for 2-5 hours, and then activating with water vapor at 750-800°C for 2-3 hours.

[0028] Preferably, step (4) further comprises the step of immersing the lignite-based honeycomb activated carbon in anhydrous ethanol containing perfluorooctyltrichlorosilane.

[0029] The present invention also provides a lignite-based honeycomb activated carbon, which is obtained by the preparation method of the lignite-based honeycomb activated carbon.

[0030] The above solution of the present invention includes at least the following beneficial effects:

[0031] (1) The preparation method of lignite-based honeycomb activated carbon of the present invention comprises the following steps: taking lignite powder, acidifying it to obtain acidified coal powder; adding organic binder and water to the acidified coal powder, mixing them evenly, and then adding a mixture of isopropyl titanate precursor solution and rosin-based quaternary ammonium salt thereto, kneading them, and mixing them evenly to obtain plastic coal slime; loading the plastic coal slime into an extrusion molding machine, extruding and molding a honeycomb blank; heat-treating the honeycomb blank to obtain lignite-based honeycomb activated carbon. The lignite-based honeycomb activated carbon obtained by the preparation method is not easy to turn white, not easy to crack, has good mechanical strength, good hydrophobicity, and good adsorption effect, and is particularly suitable for adsorbing volatile organic matter in gases with high humidity.

[0032] The method for preparing lignite-based honeycomb activated carbon first acidifies lignite powder, and uses acid to react with alkali metals (sodium, potassium, etc.) in the lignite powder, which can prevent the whitening phenomenon of the finished lignite-based honeycomb activated carbon caused by alkali metals. At the same time, the acidification treatment introduces a large number of oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface of the lignite powder, which can enhance the hydrophilicity of the lignite powder, facilitate the formation of uniformly dispersed plastic coal slime during kneading, and prevent the problems of stress concentration and easy cracking caused by uneven distribution.

[0033] The isopropyl titanate precursor solution is mixed with the acidified coal powder in the kneading stage, and reacts to generate titanium dioxide in the subsequent heat treatment stage. Since the oxygen-containing functional groups on the surface of the acidified coal powder have a higher surface energy, they are more likely to become nucleation sites for titanium dioxide, promote the crystallization and growth of titanium dioxide, and form certain physical cross-links to fill the pores and defects between the coal powder particles, reduce the adverse effects of internal defects on mechanical properties, and thus enhance the internal bonding force of the material. At the same time, the organic binder is pyrolyzed during the heat treatment process, so that the titanium dioxide forms a rough surface structure, and the high surface energy substances on the surface of the coal powder are covered by low surface energy titanium dioxide, which can enhance the hydrophobicity of the material and avoid the problem that these high surface energy substances adsorb water molecules and reduce the adsorption capacity of activated carbon.

[0034] The rosin-based quaternary ammonium salt, as a surfactant, can promote the formation of uniform plastic coal slime by acidified coal powder, isopropyl titanate precursor solution, binder, and water. More importantly, the rosin-based quaternary ammonium salt can be used as a template to form titanium dioxide in the isopropyl titanate precursor solution and improve the orderliness of the pores when pores are formed during the heat treatment process.

[0035] (2) The preparation method of lignite-based honeycomb activated carbon of the present invention, the heat treatment in step (4) includes: first maintaining at 100-150°C for 1-2 hours, then heating to 300-500°C at a rate of 2-6°C / min under the protection of an inert gas, and maintaining for 1-2 hours; then, carbonizing at 600-700°C for 2-5 hours, and then activating with water vapor at 750-800°C for 2-3 hours.

[0036] The honeycomb green body is formed in the presence of the organic binder. At 100-150° C., the honeycomb green body begins to dry gradually. Meanwhile, the isopropyl titanate precursor solution crystallizes to generate amorphous titanium dioxide, which fills the pores and defects between the acidified coal powder particles.

[0037] The temperature is raised to 300-500°C at a rate of 2-6°C / min and maintained for 1-2h. During this process, the organic binder and rosin-based quaternary ammonium salt begin to pyrolyze, while the coal powder begins to form a colloid and precipitate tar. The tar can be used as a high-temperature binder to agglomerate the coal powder, replacing the pyrolyzed organic binder to prevent the honeycomb body from cracking and collapsing. The amorphous titanium dioxide is converted into anatase titanium dioxide, which can provide higher mechanical strength, and can also reduce the cracking of the honeycomb body caused by thermal stress to a certain extent, and improve thermal stability. At the same time, the pyrolyzed organic binder and rosin-based quaternary ammonium salt leave pores in the process of converting titanium dioxide into anatase titanium dioxide, forming a highly ordered porous structure.

[0038] Finally, the honeycomb green body is carbonized at 600-700° C. for 2-5 hours, and then activated with water vapor at 750-800° C. for 2-3 hours to obtain honeycomb activated carbon. DETAILED DESCRIPTION

[0039] In the embodiments of the present invention, if the specific conditions are not specified, the conventional conditions or the conditions recommended by the manufacturer are followed. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. Raw materials of different manufacturers and models do not affect the implementation of the technical solution of the present invention and the realization of the technical effects.

[0040] In the present invention, the rosin-based quaternary ammonium salt is a product of the prior art and is prepared using the prior art. The rosin-based quaternary ammonium salts used in the following embodiments are two types, and those skilled in the art may also select other rosin-based quaternary ammonium salts according to actual conditions. The first type (hereinafter referred to as the first rosin-based quaternary ammonium salt) has a structure as shown in formula (I):

[0041]

[0042] (I)

[0043] Wherein, R has a structure as shown in formula (II):

[0044]

[0045] (II)

[0046] The first rosin-based quaternary ammonium salt can be prepared by using existing technology, for example, it can be prepared by using the method described in Chinese patent document CN102688722A.

[0047] The second type (hereinafter referred to as the second rosin-based quaternary ammonium salt) has a structure as shown in formula (III):

[0048]

[0049] (III)

[0050] The second rosin-based quaternary ammonium salt can be prepared by existing technology, for example, can be obtained by the following reaction:

[0051]

[0052] In the following examples, the lignite powder used is Xinjiang lignite, which contains alkaline components.

[0053] Example 1

[0054] The preparation method of lignite-based honeycomb activated carbon in this embodiment comprises the following steps:

[0055] (1) taking lignite powder, crushing the lignite powder to a particle size of less than 1 mm, immersing the lignite powder in an acid solution, stirring at 20° C. for 2 h, filtering, and obtaining acidified coal powder;

[0056] Wherein, the acid solution is a hydrochloric acid solution with a concentration of 4 mol / L.

[0057] (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained;

[0058] The isopropyl titanate precursor solution is a mixture of isopropyl titanate and water in a volume ratio of 1:100. The weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:6:3:5:0.4. The organic binder is hydroxyethyl cellulose. The rosin-based quaternary ammonium salt is the first rosin-based quaternary ammonium salt.

[0059] (3) The plastic coal slime in step (2) is loaded into an extruder, and extruded to form a honeycomb green body at a pressure of 13 MPa;

[0060] (4) The honeycomb blank in step (3) is first kept at 100°C for 1.5 hours, then heated to 400°C at a rate of 2°C / min under the protection of an inert gas, and kept at that temperature for 1 hour; then, carbonized at 650°C for 2 hours, and then activated with water vapor at 780°C for 3 hours to obtain lignite-based honeycomb activated carbon.

[0061] Example 2

[0062] The preparation method of lignite-based honeycomb activated carbon in this embodiment comprises the following steps:

[0063] (1) taking lignite powder, crushing the lignite powder to a particle size of less than 2 mm, immersing the lignite powder in an acid solution, stirring at 50° C. for 3 h, filtering, and obtaining acidified coal powder;

[0064] Wherein, the acid solution is a nitric acid solution with a concentration of 5 mol / L.

[0065] (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained;

[0066] The isopropyl titanate precursor solution is a mixture of isopropyl titanate and water in a volume ratio of 1:80. The weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:4:4:8:0.8. The organic binder is polyvinyl alcohol. The rosin-based quaternary ammonium salt is the second rosin-based quaternary ammonium salt.

[0067] (3) The plastic coal slime in step (2) is loaded into an extruder, and extruded to form a honeycomb green body at a pressure of 15 MPa;

[0068] (4) The honeycomb green body in step (3) is first kept at 150°C for 2 hours, then heated to 500°C at a rate of 6°C / min under the protection of an inert gas, and kept at that temperature for 2 hours; then, carbonized at 700°C for 5 hours, and then activated with water vapor at 800°C for 2 hours to obtain lignite-based honeycomb activated carbon.

[0069] Example 3

[0070] The preparation method of lignite-based honeycomb activated carbon in this embodiment comprises the following steps:

[0071] (1) taking lignite powder, crushing the lignite powder to a particle size of less than 2 mm, immersing the lignite powder in an acid solution, stirring at 35° C. for 1 hour, filtering, and obtaining acidified coal powder;

[0072] Wherein, the acid solution is one of hydrochloric acid and nitric acid; the concentration of the acid solution is 4-6 mol / L.

[0073] (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained;

[0074] The isopropyl titanate precursor solution is a mixture of isopropyl titanate and water in a volume ratio of 1:90. The weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:2:5:6:0.1. The organic binder is sodium carboxymethyl cellulose. The rosin-based quaternary ammonium salt is the first rosin-based quaternary ammonium salt.

[0075] (3) The plastic coal slime in step (2) is loaded into an extruder, and extruded to form a honeycomb green body at a pressure of 12 MPa;

[0076] (4) The honeycomb green body in step (3) is first kept at 120°C for 1 hour, then heated to 300°C at a rate of 4°C / min under the protection of an inert gas, and kept at this temperature for 1.5 hours; then, carbonized at 600°C for 3 hours, and then activated with water vapor at 750°C for 3 hours to obtain lignite-based honeycomb activated carbon.

[0077] Example 4

[0078] The preparation method of lignite-based honeycomb activated carbon in this embodiment comprises the following steps:

[0079] (1) taking lignite powder, crushing the lignite powder to a particle size of less than 0.8 mm, immersing the lignite powder in an acid solution, stirring at 30° C. for 3 h, filtering, and obtaining acidified coal powder;

[0080] Wherein, the acid solution is a hydrochloric acid solution with a concentration of 6 mol / L.

[0081] (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained;

[0082] The isopropyl titanate precursor solution is a mixture of isopropyl titanate and water in a volume ratio of 1:90. The weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:4:5:6:0.5. The organic binder is a mixture of urea-formaldehyde resin and hydroxyethyl cellulose in a weight ratio of 1:2. The rosin-based quaternary ammonium salt is the first rosin-based quaternary ammonium salt.

[0083] (3) The plastic coal slime in step (2) is loaded into an extruder, and extruded to form a honeycomb green body at a pressure of 15 MPa;

[0084] (4) The honeycomb green body in step (3) is first kept at 150°C for 2 hours, and then heated to 500°C at a rate of 6°C / min under the protection of an inert gas and kept at this temperature for 2 hours; then, carbonized at 700°C for 3 hours, and then activated with water vapor at 780°C for 3 hours to obtain lignite-based honeycomb activated carbon; and the lignite-based honeycomb activated carbon is immersed in anhydrous ethanol containing perfluorooctyltrichlorosilane for 20 minutes.

[0085] Comparative Example 1

[0086] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, the only difference is that in step (1), the step of acidifying the lignite powder is not included.

[0087] Step (1) of this comparative example is specifically as follows: taking lignite powder, and crushing the lignite powder into a particle size less than 0.8 mm.

[0088] Comparative Example 2

[0089] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, the only difference is that in step (2), the step of adding isopropyl titanate precursor solution is not included.

[0090] Step (2) of this comparative example is specifically as follows: adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding rosin-based quaternary ammonium salt thereto, kneading, and mixing evenly to obtain plastic coal slime.

[0091] Comparative Example 3

[0092] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, the only difference is that in step (2), the step of adding rosin-based quaternary ammonium salt is not included.

[0093] Step (2) of this comparative example is specifically as follows: adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding isopropyl titanate precursor solution thereto, kneading, and mixing evenly to obtain plastic coal slime.

[0094] Comparative Example 4

[0095] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the rosin-based quaternary ammonium salt is a second rosin-based quaternary ammonium salt.

[0096] Comparative Example 5

[0097] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the organic binder is hydroxyethyl cellulose.

[0098] Comparative Example 6

[0099] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the organic binder is urea-formaldehyde resin.

[0100] Comparative Example 7

[0101] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the organic binder is polyvinyl alcohol.

[0102] Comparative Example 8

[0103] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the organic binder is a mixture of urea-formaldehyde resin and polyvinyl alcohol in a weight ratio of 1:2.

[0104] Comparative Example 9

[0105] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:4:5:3:0.5.

[0106] Comparative Example 10

[0107] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, except that in step (2), the weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100:4:5:10:0.5.

[0108] Comparative Example 11

[0109] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, the only difference is that: step (1) does not include the step of acidifying the lignite powder, and in step (2), isopropyl titanate precursor solution is not added.

[0110] Comparative Example 12

[0111] The preparation method of the lignite-based honeycomb activated carbon in this comparative example is the same as that in Example 4, the only difference is that in step (4), the step of immersing the lignite-based honeycomb activated carbon in anhydrous ethanol containing perfluorooctyltrichlorosilane for 20 minutes is not included.

[0112] Step (4) of this comparative example is specifically as follows: the honeycomb blank in step (3) is first kept at 150°C for 2 hours, then heated to 500°C at a rate of 6°C / min under the protection of an inert gas, and kept at that temperature for 2 hours; then, carbonized at 700°C for 3 hours, and then activated with water vapor at 780°C for 3 hours to obtain lignite-based honeycomb activated carbon.

[0113] Effect experiment example

[0114] In order to verify the technical effect of the preparation method of lignite-based honeycomb activated carbon described in the present invention, the following experiments were conducted:

[0115] The lignite-based honeycomb activated carbon was prepared by the methods of Examples 1-4 and Comparative Examples 1-12, and the compressive strength and the methylene blue adsorption were measured. The lignite-based honeycomb activated carbon was placed at the same room temperature for 72 hours to observe the whitening of the lignite-based honeycomb activated carbon.

[0116] A dioxin generation source system is used to generate dioxin gas. The dioxin generation source system at least includes a gas source, a gas pressure reducing valve, a gas flow meter, a microdialysis pump, a micro-syringe, an atomizer, and a quartz tube. Dioxin is dissolved in an organic solvent for standby use. Using a microdialysis pump and a micro-syringe, water or a dioxin organic solvent can be injected into the atomizer at a certain speed, and the atomized gas enters the quartz tube, and the gas outlet end of the quartz tube is the sample outlet.

[0117] The lignite-based honeycomb activated carbon prepared in Examples 1-4 and Comparative Examples 1-12 were taken as samples and added to the fixed bed respectively. The fixed bed was connected to the sample outlet, and the tail gas of the fixed bed was absorbed by the tail gas absorption device. The tail gas absorption device was a toluene solution, and the tail gas flowing out of the fixed bed was discharged after absorbing dioxins by the toluene solution.

[0118] The dioxin organic solvent was injected into the nebulizer at a rate of 0.2 mL / min using a microdialysis pump and a micro-syringe. The toluene solution was collected after 30 minutes of continuous operation. The dioxin content was measured by a mass spectrometer and the first dioxin removal rate was calculated; the first dioxin removal rate = (the total amount of dioxins output by the dioxin generation source this time - the total amount of dioxins in the toluene solution) / the total amount of dioxins output by the dioxin generation source this time.

[0119] Replace the toluene solution and, under the same conditions, use a microdialysis pump and a microsyringe to inject equal volumes of water and dioxin organic solvent into the nebulizer at a rate of 0.1 mL / min, collect the toluene solution after 30 minutes of continuous operation, measure the dioxin content by mass spectrometer, and calculate the secondary dioxin removal rate; secondary dioxin removal rate = (the total amount of dioxins output by the dioxin generation source this time - the total amount of dioxins in the toluene solution) / the total amount of dioxins output by the dioxin generation source this time.

[0120] After experimentation, the results are as follows:

[0121]

[0122] According to the results of Examples 1-4 and Comparative Examples 1-12, the lignite-based honeycomb activated carbon of the present invention is not easy to turn white, has good mechanical strength, good hydrophobicity and good adsorption effect.

[0123] According to the results of Example 4 and Comparative Examples 1 and 11, acidification of lignite pulverized coal can avoid the problem of activated carbon turning white, and can significantly improve the compressive strength of lignite-based honeycomb activated carbon.

[0124] According to the results of Example 4 and Comparative Examples 2, 11, 9, and 10, the addition of the isopropyl titanate precursor solution can significantly improve the compressive strength of the lignite-based honeycomb activated carbon, and has a significant effect on the removal rate of secondary dioxins, that is, the addition of the isopropyl titanate precursor solution enhances the hydrophobicity of the lignite-based honeycomb activated carbon, and when adsorbing high-humidity dioxin gas, the adsorption performance is less affected by water vapor. However, according to the results of Comparative Examples 2 and 11, the secondary dioxin removal rate of Comparative Example 11 is less reduced than the first dioxin removal rate, which indicates that after the acidification of the lignite coal powder, if the oxygen-containing groups such as hydroxyl and carboxyl introduced are not treated with the isopropyl titanate precursor solution, the hydrophilicity of the obtained lignite-based honeycomb activated carbon will increase, and when adsorbing organic matter in high-humidity gas, the presence of water molecules will greatly weaken its adsorption capacity for organic matter such as dioxins. In comparative example 9, where the amount of isopropyl titanate precursor solution used was too small, the hydrophobicity and compressive strength were not ideal. In comparative example 10, where the amount of isopropyl titanate precursor solution used was too small, although the hydrophobicity and compressive strength were good, the adsorption capacity decreased significantly.

[0125] According to the results of Example 4 and Comparative Examples 3 and 4, the rosin-based quaternary ammonium salt has a certain influence on the mechanical strength, adsorption capacity and hydrophobicity of the obtained lignite-based honeycomb activated carbon. Compared with the second rosin-based quaternary ammonium salt, the first rosin-based quaternary ammonium salt of the Gemini surfactant has a better effect, that is, the symmetrical tricyclic phenanthrene rigid skeleton structure is more conducive to the formation of an ordered pore structure.

[0126] According to the results of Example 4 and Comparative Examples 5-8, the organic binder has a relatively small effect on the hydrophobicity of the obtained lignite-based honeycomb activated carbon, but has a greater effect on the mechanical strength and adsorption capacity. When the organic binder is a mixture of urea-formaldehyde resin and hydroxyethyl cellulose in a weight ratio of 1:2, the mechanical strength and adsorption capacity are optimal.

[0127] According to the results of Example 4 and Comparative Example 12, the perfluorooctyltrichlorosilane has a certain degree of improvement effect on the hydrophobicity of the lignite-based honeycomb activated carbon.

[0128] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are encompassed by the present invention.

Claims

1. A method for preparing lignite-based honeycomb activated carbon, characterized in that: The steps include: (1) taking lignite powder and acidifying it to obtain acidified coal powder; (2) adding an organic binder and water to the acidified coal powder in step (1), mixing them evenly, and then adding a mixture of an isopropyl titanate precursor solution and a rosin-based quaternary ammonium salt thereto, kneading and mixing until plastic coal slime is obtained; (3) loading the plastic coal slime in step (2) into an extruder to extrude and form a honeycomb blank; (4) heat treating the honeycomb blank in step (3) to obtain lignite-based honeycomb activated carbon; The heat treatment includes: first maintaining at 100-150°C for 1-2 hours, then heating to 300-500°C at a rate of 2-6°C / min under the protection of an inert gas, and maintaining for 1-2 hours; then, carbonizing at 600-700°C for 2-5 hours, and then activating with water vapor at 750-800°C for 2-3 hours.

2. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: In step (1), the acidification specifically comprises: immersing the lignite powder in an acid solution, stirring at 20-50° C. for 1-3 hours, and filtering; The acid solution is one of hydrochloric acid and nitric acid; the concentration of the acid solution is 4-6 mol / L.

3. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: Step (1) also includes the step of crushing the lignite powder to a particle size less than or equal to 2 mm.

4. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: In step (2), the isopropyl titanate precursor solution is prepared by mixing isopropyl titanate and water in a volume ratio of 1:(80-100).

5. The method for preparing lignite-based honeycomb activated carbon according to claim 4, characterized in that: In step (2), the weight ratio of the acidified coal powder, the organic binder, water, the isopropyl titanate precursor solution, and the rosin-based quaternary ammonium salt is 100: (2-6): (3-5): (5-8): (0.1-0.8).

6. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: In step (2), the organic binder is one or more of urea-formaldehyde resin, hydroxyethyl cellulose, polyvinyl alcohol, and sodium carboxymethyl cellulose.

7. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: In step (3), the extrusion molding pressure is 12-15 MPa.

8. The method for preparing lignite-based honeycomb activated carbon according to claim 1, characterized in that: Step (4) also includes the step of immersing the lignite-based honeycomb activated carbon in anhydrous ethanol containing perfluorooctyltrichlorosilane.

9. A lignite-based honeycomb activated carbon, characterized in that: The activated carbon is obtained by the preparation method of the lignite-based honeycomb activated carbon described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Hydrogenated rosin-based quaternary ammonium salt gemini surfactant and preparation method thereof

    CN102688722A

  • Activated carbon honeycomb catalyst beds and methods for the manufacture of same

    CN101472668A

  • Active carbon catalyst and preparation method and application thereof

    CN102921406A

  • Photocatalytic cellular activated carbon net

    CN104549370A

  • Method for preparing honeycomb-shaped activated carbonwith high specific surface area

    CN107235489A