A bromine-free environmentally friendly flame retardant for rubber and preparation method thereof

By using a three-source integrated flame retardant composed of phosphorus, nitrogen and carbon in polymer materials, the graft reaction of lignin with melamine and acetophosphoric acid forms a core-shell structure, the flammability and service life of polymer materials is solved. , achieving the improvement of efficient flame retardant effect and mechanical properties.

CN118580502BActive Publication Date: 2024-11-26QINGDAO PUNUOEN BIOTECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410827577.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-26
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The flammability of existing polymer materials leads to the release of toxic gases in fires, and the service life and mechanical properties of traditional flame retardants are insufficient, especially the stability and degradability of cross-linking networks of bromine-free flame retardants in polymer materials. The problem has not been effectively resolved.

Method used

A three-source integrated environmentally friendly flame retardant composed of phosphorus, nitrogen and carbon is used to form a biomass-based flame retardant similar to the core-shell structure through the grafting reaction of lignin with melamine, ethylphosphate and sulfaguanidine to form a biomass-based flame retardant similar to the core-shell structure, enhancing storage stability and reduce the possibility of degradation, while using block copolymerization structures and N-H bonds to promote interfacial compatibility and crosslinking reactions.

Benefits of technology

It achieves efficient prevention of flame spread, improves flame retardant effect and service life, while maintaining the mechanical properties of the material, reducing the orderly arrangement between molecules, and enhancing the impact toughness of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910956280000071
    Figure BDA0004910956280000071
  • Figure BDA0004910956280000081
    Figure BDA0004910956280000081
Patent Text Reader

Abstract

The invention discloses a bromine-free environmentally friendly flame retardant for rubber and a preparation method thereof. The flame retardant uses lignin as a raw material, and successively introduces melamine, ethylphosphonic acid and a self-made polymer chain to form a biomass-based flame retardant similar to a core-shell structure, thereby enhancing its storage stability, reducing the possibility of degradation of biomass-based materials in the flame retardant, and increasing the service life of the flame retardant. The flame retardant can effectively prevent the spread of flames through the synergistic flame retardant effect within the molecule, and has a good flame retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of flame retardants, and specifically relates to a bromine-free, environmentally friendly flame retardant for rubber and a preparation method thereof. Background Art

[0002] The research and application of polymer flame retardants is an important direction in the current field of materials science. The long carbon chain of polymer materials determines that their flammability is a long-standing problem. This characteristic makes polymer materials easy to release a large amount of toxic gases in a fire, which seriously threatens people's life safety. Flame retardants are designed to improve the fire resistance of polymer materials, reduce the release of smoke and toxic gases during fire, and try to maintain or improve the original performance of the materials.

[0003] In order to prevent the occurrence and spread of fire, the following four aspects can be taken into consideration: (a) reducing the heat to a temperature below that required to maintain combustion; (b) changing the degradation process of the polymer to reduce the emission of combustible volatiles; (c) isolating the flame from oxygen; (d) reducing the heat backflow to the polymer to prevent further pyrolysis. The flame retardant mechanisms currently recognized by the public are: 1. diluting the oxygen concentration by absorbing heat and producing a large amount of gas during the combustion process, thereby achieving a flame retardant effect; 2. certain flame retardants can form a non-flammable protective layer on the surface of the material to prevent the spread of flames; 3. interrupting the chain reaction in the combustion process by decomposing or capturing free radicals.

[0004] So far, the research and development of flame retardants has made significant progress, among which the research and development of bromine-free flame retardants is a direct product of the increased awareness of environmental protection in recent years. Traditional halogen (mainly bromine) flame retardants are restricted due to their potential harm to the environment, which has led to the emergence of environmentally friendly flame retardants. These new environmentally friendly flame retardants not only improve the flame retardant efficiency, but also reduce the release of smoke and toxic gases during combustion.

[0005] Patent CN108659228B provides a modified lignin flame retardant prepared by phosphating reaction and melamine grafting reaction. The flame retardant overcomes the problems of interface incompatibility and poor dispersibility, ensures that the physical and mechanical properties of the material are not affected, and is suitable for flame retardant fire protection of wood, plastic, wood-plastic composite materials and coatings. However, the degradability of the modified lignin affects the service life of the related materials. Patent CN 109957114B discloses a lignin expansion flame retardant and a preparation method thereof. The flame retardant uses hydroxymethyl lignin to react with piperazine or its derivatives and DOPO reaction intermediates to obtain a nitrogen-phosphorus synergistic lignin expansion flame retardant, which shows good flame retardant effect in polymer materials such as epoxy resins, but the reaction activity of the NH bond in the structure may be insufficient, which may damage the cross-linked network of the polymer material. Summary of the invention

[0006] The present invention provides a bromine-free environmentally friendly flame retardant for rubber and a preparation method thereof. The flame retardant is an environmentally friendly flame retardant composed of three sources of phosphorus, nitrogen and carbon. Lignin is used as a raw material, and a biomass-based flame retardant with a core-shell structure is formed by grafting reactants, thereby enhancing its storage stability, reducing the possibility of degradation after the biomass-based material is mixed with polymers such as rubber, and increasing the service life of the flame retardant.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is:

[0008] In one aspect, the present invention provides a method for preparing a bromine-free, environmentally friendly flame retardant for rubber, comprising the following steps:

[0009] S1, dissolving lignin and melamine in a 1,4-dioxane aqueous solution, adding acetic acid and formaldehyde aqueous solution, heating at 50-70° C. for 3-5 hours, slowly dripping into water, collecting the precipitate, and drying to obtain reactant 1;

[0010] S2, dissolving reactant 1, formaldehyde and ethylphosphonic acid in dimethylformamide, adjusting pH to 4.5-5.5, stirring at 60-80°C for 4-6h, adding copper acetate, continuing stirring for 4-6h, and after the stirring is completed, rotary evaporation, washing and drying are performed to obtain reactant 2;

[0011] S3, dissolving sulfaguanidine and 4,4′-biphenyldicarboxaldehyde in anhydrous ethanol, stirring at 80-90° C. for 5-7 hours to obtain reactant 3, adding reactant 2 of step S2 thereto, continuing stirring for 16-20 hours, and after the stirring is completed, rotary evaporation, washing, and drying to obtain the bromine-free environmentally friendly flame retardant for rubber.

[0012] In some embodiments, the volume concentration of the 1,4-dioxane aqueous solution in step S1 is 22-28%; the concentration of the formaldehyde aqueous solution is 35-40 wt %.

[0013] In some embodiments, the operation of collecting the precipitate in step S1 is to collect the precipitate by centrifugation, the centrifugation speed is 6500-7500 rpm, and the time is 7-13 min.

[0014] With the improvement of people's awareness of fire prevention, green and environmentally friendly halogen-free flame retardants have become a research hotspot for flame retardant products. Lignin, as a biomass polymer material, has the characteristics of being green, environmentally friendly, and renewable, and its rich carbon content is suitable as a carbon source for intumescent flame retardants. Intumescent flame retardants are generally composed of acid sources, carbon sources, and gas sources. They are generally composite flame retardants containing three elements: phosphorus, nitrogen, and carbon. They react chemically at high temperatures to form an expanded carbonized layer, thereby playing a role in heat insulation and smoke suppression. They have the advantages of high flame retardant efficiency, halogen-free and low smoke, and no corrosive gas generation. They are a research hotspot in the current flame retardant field.

[0015] The present invention combines an acid source, a carbon source and a gas source into a macromolecule through chemical synthesis to form a three-source-in-one flame retardant. During the combustion process, firstly, the organic phosphorus compound can be decomposed into pyrophosphoric acid or polyphosphoric acid, catalyzing the base material to carbonize, while releasing free radical scavengers PO· and PO2·, inhibiting the chain reaction of free radicals H· and OH·, and inhibiting the combustion process of the polymer material by quenching; secondly, the nitrogen element can generate non-flammable gas during the combustion process, achieve the flame retardant purpose by diluting the oxygen concentration, and accelerate the formation of a porous carbon layer; thirdly, the carbon compound can form a porous carbon layer on the surface of the burning polymer, and the carbon layer can play the role of heat insulation, oxygen isolation, smoke suppression and the like.

[0016] In some embodiments, the mass ratio of lignin to melamine in step S1 is 1:(0.27-0.35).

[0017] In some embodiments, the molar ratio of ethylphosphonic acid in step S2 to melamine in step S1 is (2.0-2.3):1.

[0018] In some embodiments, the mass ratio of ethylphosphonic acid to copper acetate in step S2 is 1:(1.75-2.1).

[0019] The three-in-one environmentally friendly flame retardant synthesized by the invention uses lignin as a raw material, firstly grafts melamine, and then grafts ethylphosphonic acid on the melamine. The ethylphosphonic acid not only provides a phosphorus source, but also facilitates the introduction of polymer chains in the later stage.

[0020] In some embodiments, the molar ratio of sulfaguanidine to 4,4′-biphenyldicarboxaldehyde in step S3 is (1-2.3):1.

[0021] In some embodiments, the molar ratio of ethylphosphonic acid in step S2 to 4,4′-biphenyldicarboxaldehyde in step S3 is 1:(0.45-0.50).

[0022] In some embodiments, the crystallinity of reactant 3 in step S3 is 39-48%.

[0023] The reactant 3 used in the present invention is formed into a polymer chain by sulfaguanidine and 4,4'-biphenyldicarboxaldehyde in a block form, which provides more nitrogen sources. The block copolymer structure makes the grafted phosphorus source evenly distributed in the flame retardant, which is conducive to the phosphorus source to fully play the role of catalyzing the carbonization of the matrix material and capturing free radicals under the combustion state. In addition, the polymer chain will be deposited on the surface of lignin during the reaction with ethylphosphonic acid, forming a bio-based flame retardant similar to an incompletely coated core-shell structure, which enhances its storage stability, reduces the possibility of degradation of biomass-based materials after use, and increases the service life of the flame retardant.

[0024] In addition, the NH bond contained in the flame retardant structure can undergo a cross-linking reaction with the rubber substrate structure, promoting interfacial compatibility, achieving flame retardant performance improvement without reducing its mechanical properties. And the block copolymer structure in the polymer chain reduces the crystallinity of the flame retardant and rubber mixture, reduces the orderly arrangement of molecules, and increases impact toughness. The present invention also avoids the problem of easy deformation of the rubber due to low crystallinity of the flame retardant rubber mixture by controlling the crystallinity range of the reactant 3.

[0025] Another aspect of the present invention provides a bromine-free and environment-friendly flame retardant for rubber, the yield of which is 78-85%.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention provides an environmentally friendly "three-in-one" intumescent flame retardant composed of phosphorus, nitrogen and carbon elements, which can effectively prevent the spread of flames through the synergistic flame retardant effect within the molecule and has a good flame retardant effect.

[0028] 2. The environmentally friendly flame retardant synthesized by the present invention uses lignin as a raw material, first grafted with melamine, and then grafted with ethylphosphonic acid on the melamine, wherein the ethylphosphonic acid not only provides a phosphorus source, but also facilitates the introduction of polymer chains in the later stage.

[0029] 3. The present invention forms a block polymer chain with sulfaguanidine and 4,4′-biphenyldicarboxaldehyde. The block copolymer structure allows the grafted phosphorus source to be evenly distributed in the flame retardant, which is beneficial for the phosphorus source to fully exert the role of catalyzing the carbonization of the matrix material and capturing free radicals under the combustion state; it also reduces the crystallinity, reduces the orderly arrangement between molecules, and increases the impact toughness of the composite material.

[0030] 4. The polymer provided by the present invention will be deposited on the surface of lignin during the reaction with ethylphosphonic acid, forming a bio-based flame retardant similar to an incompletely coated core-shell structure, thereby enhancing its storage stability, reducing the possibility of degradation of biomass-based materials after use, and increasing the service life of the flame retardant.

[0031] 5. The NH bond in the flame retardant structure provided by the present invention can undergo a cross-linking reaction with the rubber substrate structure, thereby promoting interfacial compatibility and achieving improved flame retardant properties without reducing its mechanical properties. DETAILED DESCRIPTION

[0032] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0033] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows:

[0034] Lignin was purchased from Hubei Qibajiu Chemical Co., Ltd.

[0035] Example 1

[0036] A method for preparing a bromine-free, environmentally friendly flame retardant for rubber comprises the following steps:

[0037] S1, dissolving 80g of lignin and 25.2g of melamine in 800mL of 25% by volume 1,4-dioxane aqueous solution, adding 120mL of acetic acid and 18mL of 37wt% formaldehyde aqueous solution, heating at 60°C for 4h, slowly dripping into 2000mL of water, collecting the precipitate by centrifugation, the centrifugal speed is 7000rpm, the time is 10min, and drying at 50°C until the weight remains unchanged, to obtain reactant 1;

[0038] S2, all reactants 1, 16 mL 37 wt% formaldehyde aqueous solution and 46.2 g ethylphosphonic acid were dissolved in 1000 mL dimethylformamide, the solution was adjusted to pH = 5 with 10 wt% hydrochloric acid solution, stirred at 70 ° C for 5 h, then 83.16 g copper acetate was added, and stirring was continued for 5 h. After stirring, dimethylformamide was removed by rotary evaporation, and washed with water 3 times, and dried at 50 ° C until the weight remained unchanged to obtain reactant 2;

[0039] S3, dissolving 63.6g of sulfaguanidine and 42g of 4,4′-biphenyldicarboxaldehyde in 2400mL of anhydrous ethanol, stirring at 85°C for 6h, then adding all the reactant 2 of step S2, continuing stirring for 18h, after the stirring is completed, rotary evaporation, washing with anhydrous ethanol three times and drying at 85°C for 12h, to obtain the bromine-free environmentally friendly rubber flame retardant.

[0040] Example 2

[0041] A method for preparing a bromine-free, environmentally friendly flame retardant for rubber comprises the following steps:

[0042] S1, dissolving 80g of lignin and 21.6g of melamine in 600mL of 20% 1,4-dioxane aqueous solution, adding 100mL of acetic acid and 14mL of 35wt% formaldehyde aqueous solution, heating at 50°C for 5h, slowly dripping into 2000mL of water, collecting the precipitate by centrifugation, the centrifugal speed is 7000rpm, the time is 10min, and drying at 50°C until the weight remains unchanged, to obtain reactant 1;

[0043] S2, all reactants 1, 12 mL 37 wt % formaldehyde aqueous solution and 37.7 g ethylphosphonic acid were dissolved in 800 mL dimethylformamide, the solution was adjusted to pH = 5 with 10 wt % hydrochloric acid solution, stirred at 60 ° C for 6 h, then 66 g copper acetate was added, and stirring was continued for 6 h. After stirring, dimethylformamide was removed by rotary evaporation, and washed with water 3 times, and dried at 50 ° C until the weight remained unchanged to obtain reactant 2;

[0044] S3, dissolving 53.6g of sulfaguanidine and 32.3g of 4,4′-biphenyldicarboxaldehyde in 2000mL of anhydrous ethanol, stirring at 80°C for 7h, then adding all the reactant 2 of step S2, continuing stirring for 20h, after the stirring is completed, rotary evaporation, washing with anhydrous ethanol three times and drying at 85°C for 12h, to obtain the bromine-free environmentally friendly rubber flame retardant.

[0045] Example 3

[0046] A method for preparing a bromine-free, environmentally friendly flame retardant for rubber comprises the following steps:

[0047] S1, dissolving 80g of lignin and 28g of melamine in 1000mL of 30% 1,4-dioxane aqueous solution, adding 150mL of acetic acid and 23mL of 40wt% formaldehyde aqueous solution, heating at 70°C for 3h, slowly dripping into 2000mL of water, collecting the precipitate by centrifugation, the centrifugal speed is 7000rpm, the time is 10min, and drying at 50°C until the weight remains unchanged, to obtain reactant 1;

[0048] S2, all reactants 1, 20 mL 37 wt% formaldehyde aqueous solution and 55.7 g ethylphosphonic acid were dissolved in 1300 mL dimethylformamide, the solution was adjusted to pH = 5 with 10 wt% hydrochloric acid solution, stirred at 80 ° C for 4 h, then 116 g copper acetate was added, and stirring was continued for 4 h. After stirring, dimethylformamide was removed by rotary evaporation, and washed with water 3 times, and dried at 50 ° C until the weight remained unchanged to obtain reactant 2;

[0049] S3, dissolving 88.7g of sulfaguanidine and 53.6g of 4,4′-biphenyldicarboxaldehyde in 3000mL of anhydrous ethanol, stirring at 90°C for 5h, then adding all the reactant 2 of step S2, continuing stirring for 16h, after the stirring is completed, rotary evaporation, washing with anhydrous ethanol three times and drying at 85°C for 12h, to obtain the bromine-free environmentally friendly rubber flame retardant.

[0050] Example 4

[0051] This embodiment provides a bromine-free environmentally friendly flame retardant for rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: 20g of melamine is used in step S1.

[0052] Example 5

[0053] This embodiment provides a bromine-free environmentally friendly flame retardant for rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: 32g of melamine is used in step S1.

[0054] Example 6

[0055] This embodiment provides a bromine-free environmentally friendly flame retardant for rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: 35.28 g of 4,4′-biphenyldicarboxaldehyde is used in step S3.

[0056] Example 7

[0057] This embodiment provides an environmentally friendly scale inhibitor for boilers and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: 48.5 g of 4,4′-biphenyldicarboxaldehyde is used in step S3.

[0058] Comparative Example 1

[0059] A method for preparing a bromine-free, environmentally friendly flame retardant for rubber comprises the following steps:

[0060] S1, dissolving 80g of lignin and 25.2g of melamine in 800mL of 25% 1,4-dioxane aqueous solution, adding 120mL of acetic acid and 18mL of 37wt% formaldehyde aqueous solution, heating at 60°C for 4h, slowly dripping into 2000mL of clean water, collecting the precipitate by centrifugation, the centrifugal speed is 7000rpm, the time is 10min, and drying at 50°C until the weight remains unchanged, to obtain reactant 1;

[0061] S2. All reactants 1, 16 mL of formaldehyde and 46.2 g of ethylphosphonic acid are dissolved in 1000 mL of dimethylformamide, the solution is adjusted to a pH value of 5 with a 10 wt % hydrochloric acid solution, stirred at 70° C. for 5 h, then 83.16 g of copper acetate is added, and stirring is continued for 5 h. After stirring, dimethylformamide is removed by rotary evaporation, and the mixture is washed with water for 3 times, and dried at 50° C. until the weight remains unchanged, thereby obtaining the bromine-free environmentally friendly flame retardant for rubber.

[0062] Performance Test:

[0063] The flame retardant prepared in the embodiment and the comparative example was mixed with the polyurethane rubber and then melt-blended for 6 minutes in an internal mixer (RM-200C Harp Electric) to obtain a composite material. In this process, the mass ratio of rubber to flame retardant was 84:16; the temperature of each zone of the internal mixer was 180°C, and the speed was 50 rpm; the polyurethane rubber was purchased from Hengshui Guangfeng Engineering Rubber and Plastic Co., Ltd.

[0064] Each composite material and polyurethane rubber were hot-pressed at 15 MPa and 185°C for 15 min using a plate vulcanizer to obtain a sample with a thickness of 3.2 mm, which was used for performance tests 1 and 2;

[0065] Each composite material and polyurethane rubber were injected using a micro injection molding machine (220° C., 8 MPa) to obtain standard mechanical specimens for performance test 3.

[0066] 1. Limiting Oxygen Index Test (LOI)

[0067] The samples were cut into 100 × 6.5 × 3.2 mm 3 The limiting oxygen index test was carried out on the specimens according to the standard GB / T2406-2015. Each sample was repeated 5 times and the average value was taken.

[0068] 2. Vertical burning test

[0069] The samples were cut into 3.2×13×100 mm 3 The specimens were subjected to vertical burning test in accordance with standard ISO-9773, and the results were graded in the following categories: VTM-0, VTM-1, VTM-2 and not applicable, representing that the flammability of the materials gradually increases.

[0070] 3. Impact strength test

[0071] The impact performance of the specimens was tested using a cantilever beam impact tester in accordance with the standard GB / T1843-96. The energy was 2.75 J at room temperature and the specimen size was 80×10×4 mm. 3 , the gap is 2mm, the test is repeated 5 times and the average value is taken.

[0072] 4. Degradability test

[0073] 3 g of each of the flame retardants prepared in the examples and comparative examples were placed outdoors at an ambient temperature of 33-38° C. and a humidity of 57%, and the time required for natural complete decomposition was tested.

[0074] The above test results are shown in Table 1.

[0075] Table 1 Performance test results

[0076]

[0077]

[0078] It can be seen from the limiting oxygen index and vertical combustion grade of the data in Table 1 that the composite materials of Examples 1-3 have good flame retardant properties. Compared with polyurethane rubber, the added flame retardant does not significantly reduce the impact resistance of the substrate while improving the flame retardant effect. It can be seen from Example 1 and Comparative Example 1 that the introduction of polymer chains can greatly improve the flame retardant effect of the flame retardant and have a certain improvement on the mechanical properties. The possible reason is that the polymer chain provides more nitrogen sources, and its block copolymer structure fully exerts the catalytic and free radical capturing effects of the phosphorus source under the combustion state. In addition, the introduction of more NH bonds promotes the cross-linking reaction between the flame retardant and the rubber substrate structure, thereby strengthening the interface compatibility and ensuring the mechanical properties; and the introduction of polymer chains can also improve the degradation resistance of the flame retardant. The possible reason is that the polymer chain will be deposited on the lignin surface during the reaction with ethylphosphonic acid, forming a bio-based flame retardant with a core-shell structure, which enhances storage stability.

[0079] From Examples 1 and 4-5, it can be seen that the incomplete modification of lignin by melamine will affect the subsequent grafting, and further affect the flame retardancy and degradation resistance of the flame retardant and the mechanical properties of the composite material; and on the basis of ensuring the complete modification of lignin, it is also necessary to avoid the capture of ethylphosphonic acid by excess melamine. From Examples 1 and 6-7, it can be seen that the change in the amount of 4,4′-biphenyldicarboxaldehyde will affect the chain length of the polymer chain and the link between the polymer chain and the lignin base, and further affect the flame retardancy and degradation resistance of the flame retardant and the mechanical properties of the composite material.

[0080] The embodiments and comparative examples described above do not impose any form of limitation on the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a bromine-free, environmentally friendly flame retardant for rubber, characterized in that: The steps include: S1. Dissolve lignin and melamine in 1,4-dioxane aqueous solution, add acetic acid and formaldehyde aqueous solution, and heat at 50-70 o C for 3-5h, slowly drip into water, collect the precipitate and dry to obtain reactant 1; S2, dissolve reactant 1, formaldehyde and ethylphosphonic acid in dimethylformamide, adjust pH to 4.5-5.5, and heat at 60-80 o C, stirring for 4-6 hours, adding copper acetate, and continuing stirring for 4-6 hours. After the stirring is completed, rotary evaporation, washing, and drying are performed to obtain reactant 2; S3, dissolve sulfaguanidine and 4,4'-biphenyl dicarboxaldehyde in anhydrous ethanol at 80-90 o C and stirred for 5-7h to obtain reactant 3, to which reactant 2 of step S2 was added, and stirring was continued for 16-20h. After the stirring was completed, rotary evaporation, washing and drying were performed to obtain the bromine-free environmentally friendly rubber flame retardant; In the step S1, the mass ratio of lignin to melamine is 1:(0.27-0.35); The molar ratio of ethylphosphonic acid in step S2 to melamine in step S1 is (2.0-2.3):1; In step S2, the mass ratio of ethylphosphonic acid to copper acetate is 1:(1.75-2.1); The molar ratio of sulfaguanidine to 4,4'-biphenyldicarboxaldehyde in step S3 is (1-2.3):1; The molar ratio of ethylphosphonic acid in step S2 to 4,4'-biphenyldicarboxaldehyde in step S3 is 1:(0.45-0.50).

2. The method for preparing a bromine-free, environmentally friendly flame retardant for rubber according to claim 1, characterized in that: In step S1, the volume concentration of the 1,4-dioxane aqueous solution is 22-28%; the concentration of the formaldehyde aqueous solution is 35-40wt%.

3. The method for preparing a bromine-free, environmentally friendly flame retardant for rubber according to claim 1, characterized in that: The operation of collecting the precipitate in step S1 is to collect the precipitate by centrifugation, the centrifugal speed is 6500-7500 rpm, and the time is 7-13 minutes.

4. The method for preparing a bromine-free, environmentally friendly flame retardant for rubber according to claim 1, characterized in that: The crystallinity of the reactant 3 in step S3 is 39-48%.

5. A bromine-free, environmentally friendly flame retardant for rubber obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The yield of the flame retardant is 78-85%.