A high temperature resistant samarium iron nitrogen permanent magnetic material and preparation method thereof
By doping cobalt, vanadium, dysprosium, and zinc into samarium-iron nitrogen permanent magnet materials, and using magnetron sputtering and modified polyamide granulation technology to form a thermally conductive layer, the durable samarium-iron nitrogen permanent magnet materials at high temperatures is solved. The problem of insufficient properties has significantly improved coerciveness and high temperature resistance, and is suitable for high temperature applications.
Patent Information
- Application Number
- CN202410794750.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The existing samarium iron nitrogen permanent magnet materials lack durability and coercivity at high temperatures, making it difficult to meet the application needs in the high temperature field.
The composition is composed of 18-20% samarium, 32-38% cobalt, 20-24% iron, 1-2% vanadium, 2-3% dysprosium, 1-2% zinc, 4-6% nitrogen. Material: High temperature resistant samarium iron nitrogen permanent magnet material is prepared by magnetron sputtering and modified polyamide granulation and injection molding. The dysprosium zinc film is used as a diffusion source for grain boundary diffusion, and triphenylamine groups are introduced into the polyamide and Carbon nanotubes are combined to form a thermally conductive layer to improve the high temperature resistance of the material.
It significantly improves the coercive force and high temperature resistance of samarium-iron nitrogen permanent magnet material, enhances the material's anti-magnetization ability and air gap magnetic tightness, adapts to the dynamic working environment of strong demagnetization, and extends the service life of the motor.
Smart Images

Figure CN118588395B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth permanent magnetic materials, in particular to a high temperature resistant samarium iron nitrogen permanent magnetic material and a preparation method thereof. Background Art
[0002] At present, the permanent magnet material with the highest magnetic properties is the rare earth NdFeB permanent magnet material, among which the maximum magnetic energy product of sintered NdFeB permanent magnet material has exceeded 56MGOe, which is very conducive to the miniaturization and lightweight of devices. In recent years, it has been widely used in wind power generation, new energy vehicles and elevators. However, NdFeB material has the disadvantage of poor high temperature resistance, which seriously limits its application in high temperature fields. In contrast, SmFeN magnets circumvent the shortcomings of NdFeB magnets such as low Curie temperature, easy oxidation and high cost, and have become a research hotspot for the new generation of rare earth permanent magnet materials.
[0003] However, Sm2Fe17Nx compounds are very likely to undergo irreversible decomposition when the temperature exceeds 550°C, so it is difficult to prepare dense magnets through traditional sintering processes. Therefore, Sm2Fe17Nx compounds are generally mixed with plastic binders such as nylon 6 and polylaurolactam at 200-300°C for granulation and injection molding to finally produce injection-molded magnets.
[0004] Generally speaking, the coercive force temperature coefficient of Sm2Fe17Nx compound magnet is about -0.5% / ℃, that is, starting from about 20℃, the coercive force decreases by 0.5% for every 1℃ increase in temperature. When the temperature rises to about 100℃, the coercive force decreases by about 40%, which will cause the motor to fail or even become dangerous. The coercive force is related to the motor's anti-demagnetization ability, that is, the overload multiple and air gap flux density and other indicators. The larger the coercive force value, the stronger the motor's anti-demagnetization ability, the larger the overload multiple, the stronger the adaptability to the strong demagnetization dynamic working environment, and the air gap flux density of the motor will also be improved.
[0005] The invention patent with announcement number CN115240946A discloses a samarium iron nitrogen-based anisotropic permanent magnet material and its preparation method and application. Metal cobalt is doped into the traditional samarium iron nitrogen magnet to replace part of the iron to improve the high-temperature stability of the magnet material. However, doping only a small amount of cobalt cannot significantly improve the high temperature resistance and coercive force.
[0006] It can be seen that researching and preparing a high-temperature resistant samarium iron nitrogen permanent magnet material is still an urgent problem that technical personnel in this field need to solve. Summary of the invention
[0007] The object of the present invention is to provide a high temperature resistant samarium iron nitrogen permanent magnet material and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a high temperature resistant samarium iron nitrogen permanent magnet material, comprising the following components in mass percentage: 18-20% samarium, 32-38% cobalt, 20-24% iron, 1-2% vanadium, 2-3% dysprosium, 1-2% zinc, 4-6% nitrogen, and the rest is modified polyamide.
[0009] Preferably, the samarium source, cobalt source, vanadium source and iron source are samarium-iron alloy and iron-cobalt alloy; the mass percentage of each component in the samarium-iron alloy is: 20-25% samarium, and the rest is iron; the mass percentage of each component in the iron-cobalt alloy is: 49-52% cobalt, 0-10% vanadium, and the rest is iron.
[0010] Preferably, the high temperature resistant samarium iron nitrogen permanent magnet material is obtained by magnetron sputtering magnetic powder, granulating it with modified polyamide and injection molding it.
[0011] Preferably, the magnetron sputtering uses a dysprosium zinc film as a diffusion source; the thickness of the dysprosium zinc film is 2 to 4 μm.
[0012] Preferably, the modified polyamide is prepared by introducing triphenylamine groups into the main chain of polyamide and then compounding with a small amount of carbon nanotubes.
[0013] Preferably, the method for preparing the high temperature resistant samarium iron nitrogen permanent magnet material comprises the following specific steps:
[0014] S1. Place the samarium iron alloy and the iron-cobalt alloy in a nitriding furnace, raise the temperature to 530-540°C in an ammonia atmosphere, and perform the nitriding reaction for 12-24 hours. After cooling in the furnace, crush the alloy to obtain magnetic powder.
[0015] S2. The magnetic powder is subjected to magnetron sputtering, and after the magnetron sputtering, it is transferred to a high vacuum furnace for heat treatment to obtain magnetic powder after magnetron sputtering;
[0016] S3. The chlorinated carbon nanotubes and dimethyl sulfoxide are mixed in a mass ratio of 1:8 to 10, the temperature is raised to 60 to 70°C, and after ultrasonic dispersion, 0.2 to 0.4 times the mass of the chlorinated carbon nanotubes, 80 to 100 times the mass of the chlorinated carbon nanotubes, and 2.2 to 2.8 times the mass of the chlorinated carbon nanotubes are added with triphenylamine polyamide, and the reaction is carried out at room temperature for 24 hours, and the mixture is filtered and washed with deionized water for 3 to 5 times, and finally vacuum dried and ground to obtain a modified polyamide;
[0017] S4. The magnetic powder after magnetron sputtering is mixed with modified polyamide in a mass ratio of 4:0.2-1 for granulation and injection molding. The temperature during granulation is 180-220°C and the temperature during injection molding is 240-280°C to obtain a high-temperature resistant samarium iron nitrogen permanent magnet material.
[0018] Preferably, in the above step S2., during magnetron sputtering, the power is 80-120 W, the gas pressure is 1-1.2 Pa, the argon gas flow is 40-50 sccm, and the target-substrate distance is 8-10 mm.
[0019] Preferably, in the above step S2., during grain boundary diffusion, the gas pressure is 10 -4 Pa, the diffusion temperature is 600-900℃, the temperature during grain boundary diffusion is 850-950℃, and the time is 2-6h.
[0020] Preferably, in the above step S3., the preparation method of triphenylamine polyamide is: under a nitrogen atmosphere, p-phenylenediamine, p-fluoronitrobenzene, triethylamine and dimethyl sulfoxide are mixed in a mass ratio of 1-1.2:3:2:18-20, heated to 90-92°C, reacted for 6-7h, cooled to room temperature and precipitated with ice water, then 4-6 times the mass of p-phenylenediamine dioxane and 3-4 times the mass of p-phenylenediamine ethanol are added, heated to 80-90°C again, stirred evenly, palladium carbon with a mass of 0.14-0.16 times the mass of p-phenylenediamine is added, and p-phenylenediamine is added dropwise at a rate of 1-3mL / min. Hydrazine hydrate with a mass fraction of 85% is refluxed for 20 to 28 hours, filtered while hot and distilled with water, and then cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone are added, and the mass ratio of p-phenylenediamine, cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone is 5:0.18-0.2:0.15:1:0.5:2.4-2.8, the temperature is raised to 115-125°C, the reaction is carried out for 3 to 4 hours, the material is cooled and discharged in anhydrous ethanol, filtered and washed with deionized water, methanol and ethanol respectively to obtain triphenylamine polyamide.
[0021] Preferably, in the above step S3., the preparation method of the chlorinated carbon nanotubes is: mix carboxylated multi-walled carbon nanotubes, thionyl chloride and dimethylformamide in a mass ratio of 0.1:10:0.2-0.4, heat to 68-72°C, stir and react at 400-800 rpm for 20-28 hours, and distill under reduced pressure to obtain chlorinated carbon nanotubes.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] The high temperature resistant samarium iron nitrogen permanent magnetic material of the present invention is prepared by magnetron sputtering magnetic powder, granulating with modified polyamide and injection molding;
[0024] The magnetic powder includes samarium, iron, copper, cobalt, vanadium, dysprosium, zinc and nitrogen. The raw materials are nitrided to obtain magnetic powder, and then magnetron sputtering is performed; a certain amount of cobalt, vanadium, dysprosium and zinc are doped into the samarium iron nitrogen permanent magnet material to ensure the intrinsic coercive force and high temperature resistance of the permanent magnet material. During magnetron sputtering, a dysprosium zinc film is used as a diffusion source, and a metal film is first deposited on the surface of the magnet. Then, through grain boundary diffusion treatment, dysprosium and zinc diffuse through the grain boundaries inside the magnet and replace a part of the metal in the magnetic powder. They can be distributed in the area near the grains and the nucleation epitaxial layer, playing a demagnetization coupling role. The dysprosium and zinc diffused into the nucleation epitaxial layer form a new shell structure, which can improve the anisotropy field of the main phase grains and the area near the grain boundaries and prevent the formation of reverse magnetization nuclei, thereby improving the coercive force of the magnet material;
[0025] The modified polyamide is prepared by introducing triphenylamine groups into the main chain of polyamide and then compounding it with a small amount of carbon nanotubes; the triphenylamine groups are introduced into the main chain of polyamide to form a modified polyamide with a long main chain structure, thereby enhancing the rigidity and thus the heat resistance of the modified polyamide, and then compounding it with a small amount of carbon nanotubes, and by virtue of the continuity of the carbon nanotubes in space, the heat dissipation of the modified polyamide is enhanced, thereby enhancing the high temperature resistance of the permanent magnet material; the magnetic powder after magnetron sputtering is granulated with the modified polyamide and injection molded, and the modified polyamide forms a new shell structure with the dysprosium and zinc diffused into the nucleation epitaxial layer, forming a thermal conductive layer, thereby enhancing the heat dissipation of the permanent magnet material, and a high temperature resistant samarium iron nitrogen permanent magnet material can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a microscopic image of the high temperature resistant samarium iron nitrogen permanent magnet material prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] The mass percentages of the components in the samarium-iron alloy used in this embodiment and the comparative example are: 24% samarium and the rest iron, and the mass percentages of the components in the iron-cobalt alloy are: 50% cobalt, 5% vanadium, and the rest iron.
[0029] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high temperature resistant samarium iron nitrogen permanent magnet materials prepared in the examples and comparative examples as follows:
[0030] Coercive force: The high temperature resistant samarium iron nitrogen permanent magnet materials prepared in the examples and comparative examples were tested for intrinsic coercive force according to GB / T3217.
[0031] High temperature resistance: The high temperature resistant samarium iron nitrogen permanent magnet materials prepared in the same embodiment and comparative example were saturated magnetized, and then the magnetic flux before aging was measured at room temperature. Then, they were placed on a 1mm iron sheet and kept in an oven at 150°C for 1 hour. After cooling to room temperature, the magnetic flux after aging was measured, and then the high temperature resistance irreversible loss was calculated.
[0032] Example 1
[0033] The present embodiment includes the following components by mass: 20% samarium, 12% cobalt, 48% iron, 1% vanadium, 2% dysprosium, 1% zinc, 2% nitrogen, and the rest is modified polyamide;
[0034] The preparation method of the high temperature resistant samarium iron nitrogen permanent magnet material in this embodiment is as follows:
[0035] S1. The samarium iron alloy and the iron-cobalt alloy are placed in a nitriding furnace, heated to 530°C in an ammonia atmosphere, and subjected to nitriding reaction for 12 hours. The alloy is then crushed after cooling in the furnace to obtain magnetic powder;
[0036] S2. The magnetic powder was subjected to magnetron sputtering. During magnetron sputtering, a 2 μm dysprosium zinc film was used as the diffusion source, the power was 80 W, the gas pressure was 1 Pa, the argon gas flow was 40 sccm, and the target-substrate distance was 8 mm. After the magnetron sputtering, the magnetic powder was transferred to a high vacuum furnace for grain boundary diffusion treatment. During grain boundary diffusion, the gas pressure was 10 -4 Pa, diffusion temperature is 600℃, temperature of grain boundary diffusion is 850℃, time is 2h, magnetic powder after magnetron sputtering is obtained;
[0037] S3. Under a nitrogen atmosphere, p-phenylenediamine, p-fluoronitrobenzene, triethylamine and dimethyl sulfoxide were mixed in a mass ratio of 1:3:2:18, heated to 90°C, reacted for 6 hours, cooled to room temperature and precipitated with ice water, then 4 times the mass of p-phenylenediamine dioxane and 3 times the mass of p-phenylenediamine ethanol were added, heated to 80°C again, stirred evenly, palladium carbon was added in an amount of 0.14 times the mass of p-phenylenediamine, and hydrazine hydrate with a mass fraction of 85% of p-phenylenediamine was added dropwise at a rate of 1 mL / min, refluxed for 20 hours, filtered while hot and distilled with water, and then cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone were added, and the mass ratio of p-phenylenediamine, cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone was 5:0.18:0.15:1:0. .5:2.4, heat to 115°C, react for 3h, cool the material and put it into anhydrous ethanol, filter and wash with deionized water, methanol and ethanol respectively to obtain triphenylamine polyamide; mix carboxylated multi-walled carbon nanotubes, thionyl chloride and dimethylformamide in a mass ratio of 0.1:10:0.2, heat to 68°C, stir and react at 400rpm for 20h, and distill under reduced pressure to obtain chlorinated carbon nanotubes; mix chlorinated carbon nanotubes and dimethyl sulfoxide in a mass ratio of 1:8, heat to 60°C, ultrasonically disperse evenly, add 0.2 times the mass of chlorinated carbon nanotubes pyridine, 80 times the mass of chlorinated carbon nanotubes dimethyl sulfoxide, and 2.2 times the mass of chlorinated carbon nanotubes triphenylamine polyamide, react at room temperature for 24h, filter and wash with deionized water 3 times, finally vacuum dry and grind to obtain modified polyamide;
[0038] S4. The magnetic powder after magnetron sputtering is mixed with modified polyamide in a mass ratio of 4:0.2 for granulation and injection molding. The temperature during granulation is 180°C and the temperature during injection molding is 240°C to obtain a high-temperature resistant samarium iron nitrogen permanent magnet material.
[0039] Example 2
[0040] The present embodiment includes the following components by mass: 19% samarium, 10% cobalt, 50% iron, 1.5% vanadium, 2.5% dysprosium, 2% zinc, 3% nitrogen, and the remainder is modified polyamide;
[0041] The preparation method of the high temperature resistant samarium iron nitrogen permanent magnet material in this embodiment is as follows:
[0042] S1. The samarium iron alloy and the iron-cobalt alloy are placed in a nitriding furnace, heated to 535°C in an ammonia atmosphere, and subjected to nitriding reaction for 18 hours. The alloy is then crushed after cooling in the furnace to obtain magnetic powder;
[0043] S2. The magnetic powder was subjected to magnetron sputtering. During magnetron sputtering, a 3 μm dysprosium zinc film was used as the diffusion source, the power was 100 W, the gas pressure was 1.1 Pa, the argon gas flow was 45 sccm, and the target-substrate distance was 9 mm. After the magnetron sputtering, the magnetic powder was transferred to a high vacuum furnace for grain boundary diffusion treatment. During grain boundary diffusion, the gas pressure was 10 -4 Pa, diffusion temperature is 750℃, temperature of grain boundary diffusion is 900℃, time is 4h, and magnetic powder after magnetron sputtering is obtained;
[0044] S3. Under a nitrogen atmosphere, p-phenylenediamine, p-fluoronitrobenzene, triethylamine and dimethyl sulfoxide were mixed in a mass ratio of 1.1:3:2:19, heated to 91°C, reacted for 6.5 hours, cooled to room temperature and precipitated with ice water, and then 5 times the mass of p-phenylenediamine dioxane and 3.5 times the mass of p-phenylenediamine ethanol were added, and the temperature was raised to 85°C again. After stirring evenly, palladium carbon was added at a mass fraction of 0.15 times the mass of p-phenylenediamine, and hydrazine hydrate with a mass fraction of 85% of p-phenylenediamine was added dropwise at a rate of 2 mL / min. The reaction was refluxed for 24 hours, filtered while hot and distilled with water, and cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone were added. The mass ratio of p-phenylenediamine, cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone was 5:0.19:0.15:1 :0.5:2.6, heated to 120°C, reacted for 3.5h, cooled and discharged in anhydrous ethanol, filtered and washed with deionized water, methanol and ethanol respectively to obtain triphenylamine polyamide; carboxylated multi-walled carbon nanotubes, thionyl chloride and dimethylformamide were mixed in a mass ratio of 0.1:10:0.3, heated to 70°C, stirred and reacted at 600rpm for 24h, and distilled under reduced pressure to obtain chlorinated carbon nanotubes; chlorinated carbon nanotubes and dimethyl sulfoxide were mixed in a mass ratio of 1:9, heated to 65°C, ultrasonically dispersed uniformly, and 0.3 times the mass of chlorinated carbon nanotubes pyridine, 90 times the mass of chlorinated carbon nanotubes dimethyl sulfoxide, and 2.6 times the mass of chlorinated carbon nanotubes triphenylamine polyamide were added, reacted at room temperature for 24h, filtered and washed with deionized water 4 times, and finally vacuum dried and ground to obtain modified polyamide;
[0045] S4. The magnetic powder after magnetron sputtering is mixed with modified polyamide in a mass ratio of 4:0.6 for granulation and injection molding. The temperature during granulation is 200°C and the temperature during injection molding is 260°C to obtain a high-temperature resistant samarium iron nitrogen permanent magnet material.
[0046] Example 3
[0047] The present embodiment includes the following components by mass: 20% samarium, 8% cobalt, 48% iron, 2% vanadium, 3% dysprosium, 2% zinc, 4% nitrogen, and the rest is modified polyamide;
[0048] The preparation method of the high temperature resistant samarium iron nitrogen permanent magnet material in this embodiment is as follows:
[0049] S1. The samarium iron alloy and the iron-cobalt alloy are placed in a nitriding furnace, heated to 540°C in an ammonia atmosphere, and subjected to nitriding reaction for 24 hours. The alloy is then crushed after cooling in the furnace to obtain magnetic powder;
[0050] S2. The magnetic powder was subjected to magnetron sputtering. During magnetron sputtering, a 4 μm dysprosium zinc film was used as the diffusion source, the power was 120 W, the gas pressure was 1.2 Pa, the argon gas flow was 50 sccm, and the target-substrate distance was 10 mm. After the magnetron sputtering, the magnetic powder was transferred to a high vacuum furnace for grain boundary diffusion treatment. During grain boundary diffusion, the gas pressure was 10 -4 Pa, diffusion temperature is 900℃, temperature during grain boundary diffusion is 950℃, time is 6h, and magnetic powder after magnetron sputtering is obtained;
[0051] S3. Under a nitrogen atmosphere, p-phenylenediamine, p-fluoronitrobenzene, triethylamine and dimethyl sulfoxide were mixed in a mass ratio of 1.2:3:2:20, heated to 92°C, reacted for 7 hours, cooled to room temperature and precipitated with ice water, and then 6 times the mass of p-phenylenediamine dioxane and 4 times the mass of p-phenylenediamine ethanol were added, and the temperature was raised to 90°C again. After stirring evenly, palladium carbon was added at a mass fraction of 0.16 times the mass of p-phenylenediamine, and hydrazine hydrate with a mass fraction of 85% of p-phenylenediamine was added dropwise at a rate of 3 mL / min. The reaction was refluxed for 28 hours, filtered while hot and distilled with water, and cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone were added. The mass ratio of p-phenylenediamine, cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone was 5:0.2:0.15:1:0. .5:2.8, heated to 125°C, reacted for 4h, cooled and discharged into anhydrous ethanol, filtered and washed with deionized water, methanol and ethanol respectively to obtain triphenylamine polyamide; carboxylated multi-walled carbon nanotubes, thionyl chloride and dimethylformamide were mixed in a mass ratio of 0.1:10:0.4, heated to 72°C, stirred and reacted at 800rpm for 28h, and distilled under reduced pressure to obtain chlorinated carbon nanotubes; chlorinated carbon nanotubes and dimethyl sulfoxide were mixed in a mass ratio of 1:10, heated to 70°C, ultrasonically dispersed evenly, and then 0.4 times the mass of chlorinated carbon nanotubes of pyridine, 100 times the mass of chlorinated carbon nanotubes of dimethyl sulfoxide, and 2.8 times the mass of chlorinated carbon nanotubes of triphenylamine polyamide were added, reacted at room temperature for 24h, filtered and washed with deionized water 5 times, and finally vacuum dried and ground to obtain modified polyamide;
[0052] S4. The magnetic powder after magnetron sputtering is mixed with modified polyamide in a mass ratio of 4:1 for granulation and injection molding. The temperature during granulation is 220°C and the temperature during injection molding is 280°C to obtain a high-temperature resistant samarium iron nitrogen permanent magnet material.
[0053] Comparative Example 1
[0054] The composition of Comparative Example 1 is the same as that of Example 2. The difference between the preparation method of the high temperature resistant samarium iron nitrogen permanent magnetic material and that of Example 2 is that magnetron sputtering is not performed, and the magnetic powder and the modified polyamide are directly granulated and injection molded.
[0055] Comparative Example 2
[0056] The composition of comparative example 2 is the same as that of example 2. The difference between the preparation method of the high temperature resistant samarium iron nitrogen permanent magnet material and that of example 2 is that the modified polyamide is only prepared by compounding polyamide with a small amount of carbon nanotubes.
[0057] Comparative Example 3
[0058] The composition of Comparative Example 3 is the same as that of Example 2. The difference between the preparation method of the high temperature resistant samarium iron nitrogen permanent magnetic material and that of Example 2 is that the magnetic powder is subjected to magnetron sputtering, granulated with polyamide and injection molded to obtain the material.
[0059] Comparative Example 4
[0060] The composition of Comparative Example 4 is the same as that of Example 2. The difference between the preparation method of the high temperature resistant samarium iron nitrogen permanent magnet material and that of Example 2 is that magnetron sputtering is not performed, and the magnetic powder and polyamide are directly granulated and injection molded.
[0061] Effect example
[0062] Table 1 below shows the performance analysis results of high temperature resistant samarium iron nitrogen permanent magnet materials prepared by using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4:
[0063] Table 1
[0064]
[0065]
[0066] By comparing the experimental data of the embodiment and the comparative example in Table 1, it can be clearly found that the high temperature resistant samarium iron nitrogen permanent magnet materials prepared by using embodiments 1, 2 and 3 have good coercive force and high temperature resistance.
[0067] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 4, it can be found that when preparing high-temperature resistant samarium iron nitrogen permanent magnet materials, using dysprosium zinc film as the diffusion source of magnetron sputtering, a layer of metal film can be deposited on the surface of the magnet, and then through grain boundary diffusion treatment, dysprosium and zinc can diffuse at the grain boundaries inside the magnet and replace a part of the metal in the magnetic powder. They can be distributed in the area near the grains and the nucleation epitaxial layer, playing a demagnetizing coupling role, and the dysprosium and zinc diffused into the nucleation epitaxial layer form a new shell structure, which can increase the anisotropy field of the main phase grains and the area near the grain boundaries and prevent the formation of reverse magnetization nuclei, thereby improving the coercive force of the magnet material.
[0068] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 2, Comparative Example 3, Comparative Example 4, it can be found that after the triphenylamine group is introduced into the main chain of the polyamide, the modified polyamide prepared by compounding with a small amount of carbon nanotubes, the modified polyamide with high heat resistance is compounded with a small amount of carbon nanotubes, and the heat dissipation of the modified polyamide is enhanced by virtue of the continuity of the carbon nanotubes in space, thereby enhancing the high temperature resistance of the permanent magnet material; the magnetic powder after magnetron sputtering is granulated with the modified polyamide and injection molded, the modified polyamide forms a new shell structure with the dysprosium and zinc diffused into the nucleation epitaxial layer, forming a thermal conductive layer, enhancing the heat dissipation of the permanent magnet material, and a high temperature resistant samarium iron nitrogen permanent magnet material can be obtained.
[0069] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A high temperature resistant samarium iron nitrogen permanent magnet material, characterized in that: The invention comprises the following components in percentage by mass: 18-20% of samarium, 6-12% of cobalt, 48-51% of iron, 0-2% of vanadium, 2-3% of dysprosium, 1-2% of zinc, 2-4% of nitrogen, and the rest is modified polyamide.
2. The high temperature resistant samarium iron nitrogen permanent magnet material according to claim 1, characterized in that: The samarium source, cobalt source, vanadium source and iron source are samarium-iron alloy and iron-cobalt alloy; the mass percentage of each component in the samarium-iron alloy is: 20-25% samarium, and the rest is iron; the mass percentage of each component in the iron-cobalt alloy is: 49-52% cobalt, 0-10% vanadium, and the rest is iron.
3. The high temperature resistant samarium iron nitrogen permanent magnet material according to claim 1, characterized in that: The high temperature resistant samarium iron nitrogen permanent magnetic material is prepared by subjecting magnetic powder to magnetron sputtering, granulating with modified polyamide and injection molding.
4. The high temperature resistant samarium iron nitrogen permanent magnet material according to claim 3, characterized in that: The magnetron sputtering uses the dysprosium zinc film as a diffusion source; the thickness of the dysprosium zinc film is 2-4 μm.
5. The high temperature resistant samarium iron nitrogen permanent magnet material according to claim 1, characterized in that: The modified polyamide is prepared by introducing triphenylamine groups into the main chain of the polyamide and then compounding with a small amount of carbon nanotubes.
6. A method for preparing the high temperature resistant samarium iron nitrogen permanent magnetic material as claimed in claim 1, characterized in that: The specific steps include: S1. Place the samarium iron alloy and the iron-cobalt alloy in a nitriding furnace, raise the temperature to 530-540°C in an ammonia atmosphere, and perform the nitriding reaction for 12-24 hours. After cooling in the furnace, crush the alloy to obtain magnetic powder. S2. The magnetic powder is subjected to magnetron sputtering, and after the magnetron sputtering is completed, it is transferred to a high vacuum furnace for grain boundary diffusion treatment to obtain magnetic powder after magnetron sputtering; S3. The chlorinated carbon nanotubes and dimethyl sulfoxide are mixed in a mass ratio of 1:8 to 10, the temperature is raised to 60 to 70°C, and after ultrasonic dispersion, 0.2 to 0.4 times the mass of the chlorinated carbon nanotubes, 80 to 100 times the mass of the chlorinated carbon nanotubes, and 2.2 to 2.8 times the mass of the chlorinated carbon nanotubes are added with triphenylamine polyamide, and the reaction is carried out at room temperature for 24 hours, and the mixture is filtered and washed with deionized water for 3 to 5 times, and finally vacuum dried and ground to obtain a modified polyamide; S4. The magnetic powder after magnetron sputtering is mixed with modified polyamide in a mass ratio of 4:0.2-1 for granulation and injection molding. The temperature during granulation is 180-220°C and the temperature during injection molding is 240-280°C to obtain a high-temperature resistant samarium iron nitrogen permanent magnet material.
7. The method for preparing a high temperature resistant samarium iron nitrogen permanent magnetic material according to claim 6, characterized in that: In the above step S2.: during magnetron sputtering, the power is 80-120 W, the gas pressure is 1-1.2 Pa, the argon gas flow is 40-50 sccm, and the target-substrate distance is 8-10 mm.
8. The method for preparing a high temperature resistant samarium iron nitrogen permanent magnetic material according to claim 6, characterized in that: In the above step S2.: during grain boundary diffusion, the gas pressure is 10 -4 Pa, the diffusion temperature is 600-900℃, the temperature during grain boundary diffusion is 850-950℃, and the time is 2-6h.
9. The method for preparing a high temperature resistant samarium iron nitrogen permanent magnetic material according to claim 6, characterized in that: In the above step S3.: the preparation method of triphenylamine polyamide is: under a nitrogen atmosphere, p-phenylenediamine, p-fluoronitrobenzene, triethylamine and dimethyl sulfoxide are mixed in a mass ratio of 1-1.2:3:2:18-20, heated to 90-92°C, reacted for 6-7h, cooled to room temperature and precipitated with ice water, then 4-6 times the mass of p-phenylenediamine dioxane and 3-4 times the mass of p-phenylenediamine ethanol are added, heated to 80-90°C again, stirred evenly, palladium carbon is added in an amount of 0.14-0.16 times the mass of p-phenylenediamine, and p-phenylenediamine is added dropwise at a rate of 1-3mL / min. Hydrazine hydrate with a concentration of 85% is refluxed for 20 to 28 hours, filtered while hot and distilled with water, and then cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone are added, and the mass ratio of p-phenylenediamine, cyclohexanedicarboxylic acid, calcium oxide, triphenyl phosphite, pyridine and N-methyl-2-pyrrolidone is 5:0.18 to 0.2:0.15:1:0.5:2.4 to 2.8, the temperature is raised to 115 to 125°C, the reaction is carried out for 3 to 4 hours, the material is cooled and discharged in anhydrous ethanol, filtered and washed once with deionized water, methanol and ethanol in sequence to obtain triphenylamine polyamide.
10. The method for preparing a high temperature resistant samarium iron nitrogen permanent magnetic material according to claim 6, characterized in that: In the above step S3.: the preparation method of chlorinated carbon nanotubes is: carboxylated multi-walled carbon nanotubes, thionyl chloride and dimethylformamide are mixed in a mass ratio of 0.1:10:0.2-0.4, heated to 68-72°C, stirred at 400-800 rpm for 20-28 hours, and distilled under reduced pressure to obtain chlorinated carbon nanotubes.