A catalyst for acetaldehyde condensation reaction and its preparation method and application
By using solid catalysts of magnesium oxide and elements such as lanthanum, germanium, and zirconium, combined with solid carriers of chitosan and glucose, the problems of catalyst recovery and by-product control are solved, the efficiency and safety of the acetaldehyde condensation reaction are improved, and the cost of the acetaldehyde condensation reaction is reduced. production costs.
Patent Information
- Application Number
- CN202411081225.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The catalyst in the existing acetaldehyde condensation reaction is difficult to recover, resulting in a waste of resources. By-products are numerous and difficult to control, affecting product purity and safety. The reaction process is complex, resulting in high production costs.
A solid catalyst is used, with magnesium oxide as the active component, lanthanum, germanium, and zirconium as auxiliaries, magnesium salts and aluminum salts as carriers, and chitosan and glucose added to form appropriate void structures and mechanical properties to improve catalytic efficiency and selection. properties and applied in fixed bed reactors.
It achieves efficient recovery of catalysts and reduction of by-products, improves the service life and catalytic efficiency of the catalyst, reduces production costs, and ensures the high purity and safety of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a catalyst for acetaldehyde condensation reaction and a preparation method and application thereof. Background Art
[0002] 3-Hydroxybutyraldehyde is a colorless and transparent viscous liquid that is miscible with water, acetone, ethanol and ether. It can be produced by the condensation of two acetaldehyde molecules. 3-Hydroxybutyraldehyde is a basic raw material for chemical products. For example, crotonaldehyde prepared by dehydration of 3-hydroxybutyraldehyde can be widely used in polymers and synthetic resins. 3-Hydroxybutyraldehyde can also be oxidized in liquid phase to produce 3-hydroxybutyric acid, an important monomer of degradable plastics (polyhydroxybutyrate). In addition, 3-Hydroxybutyraldehyde can also be hydrogenated to produce 1,3-butanediol. 1,3-Butanediol is mainly used to synthesize polyester resins and alkyd resins. It can also be used as a humectant and softener for textiles, tobacco and paper. It is also widely used as a moisturizer in cosmetics such as lotions, emulsions and toothpastes. 1,3-Butanediol has a good antibacterial effect and has been used as an antibacterial agent for cheese or meat.
[0003] Acetaldehyde can undergo liquid-phase aldol condensation reaction under the catalytic action of NaOH solution. The industrial history of this reaction can even be traced back to the 1920s. Its basic technical characteristics are: using NaOH solution as a catalyst, liquid-phase reaction, the degree of condensation reaction is mainly controlled by the contact reaction time of NaOH solution and acetaldehyde solution, and further condensation reaction needs to be stopped by adding acetic acid to neutralize the catalytic action of NaOH.
[0004] China's invention patent (CN100450986C) discloses a method for preparing 1,3-butanediol, firstly preparing 3-hydroxybutyraldehyde by adding a small amount of carboxylic acid to sodium hydroxide, and then hydrogenating to prepare 1,3-butanediol. China's invention patent (CN105585448A), China's invention patent (CN110790634A), China's invention patent (CN206396080U) and China's invention patent (CN208883742U) disclose a process of using acetaldehyde as a raw material, first condensing 3-hydroxybutyraldehyde under the action of an alkaline catalyst, and then preparing 1,3-butanediol by a two-step hydrogenation process. The above patents all use intermittent kettle reactors and liquid alkalis (such as NaOH, KOH, LiOH, trimethylamine and triethylamine, etc.) as catalysts. However, due to the high viscosity of 3-hydroxybutyraldehyde and its easy dehydration when in contact with the catalyst for a long time or at high temperature, further purification is very difficult, and the subsequent product refining process is complicated and the production cost is increased, which seriously affects the purity and price of the product. In addition, the catalyst cannot be effectively recovered during the reaction, resulting in a waste of the catalyst. At the same time, a large amount of salt substances will be generated during the condensation reaction. If not immediately processed, it will block the catheter and easily cause production safety problems. Summary of the invention
[0005] The present invention provides a catalyst for acetaldehyde condensation reaction, a preparation method and an application thereof. The catalyst provided by the present invention is a solid catalyst, which has high catalytic efficiency and few reaction by-products, and can be applied in a fixed bed reactor and can be recovered.
[0006] In order to achieve the above object, the present invention provides a catalyst for acetaldehyde condensation reaction, comprising a carrier, an active component and a catalyst promoter; the active component is magnesium oxide; the catalyst promoter is one or more of lanthanum, germanium and zirconium; the carrier is prepared from magnesium salt and aluminum salt, and chitosan and / or glucose is added during the preparation of the carrier;
[0007] The molar ratio of magnesium to aluminum in the magnesium salt and aluminum salt is 1:1-4; the amount of chitosan and / or glucose added is 10%-20% of the total mass of the magnesium salt and aluminum salt; the molar ratio of the magnesium salt to the catalyst additive is 1:0.02-0.06;
[0008] The magnesium salt is one or more of magnesium citrate, magnesium nitrate and magnesium acetate; the aluminum salt is aluminum nitrate and / or aluminum citrate.
[0009] The present invention provides a method for preparing the catalyst for acetaldehyde condensation reaction described in the above scheme, comprising the following steps:
[0010] 1) mixing a magnesium salt solution, an aluminum salt solution, a chitosan and / or glucose solution, and an alkali solution to obtain a mixed solution;
[0011] 2) reacting, filtering, washing to neutrality and calcining the mixed solution in sequence to obtain a carrier with magnesium oxide as an active component;
[0012] 3) Loading the precursor of the catalyst promoter onto the carrier, and sequentially drying, calcining and tableting to obtain the catalyst; the precursor of the catalyst promoter is one or more of lanthanum nitrate, zirconium nitrate and germanium nitrate.
[0013] Preferably, the base in step 1) is one or more of sodium hydroxide, potassium hydroxide, monoethanolamine and ammonia water; the amount of the base used is 1.2 to 2.2 times the sum of the amounts of magnesium and aluminum elements.
[0014] Preferably, in step 2), the reaction temperature is 80-150° C. and the reaction time is 5-15 h; the calcination temperature is 400-600° C. and the reaction time is 4-10 h.
[0015] Preferably, in step 3), the precursor of the catalyst promoter is loaded on the carrier by impregnation; the impregnation time is 4 to 10 hours.
[0016] Preferably, in step 3), the drying temperature is 60-140° C., and the time is 6-24 h; the calcination temperature is 400-600° C., and the time is 4-10 h.
[0017] The present invention provides the use of any one of the above-mentioned catalysts in the preparation of 3-hydroxybutyraldehyde by acetaldehyde condensation reaction, wherein the condensation reaction is carried out in a fixed bed.
[0018] Preferably, the reaction temperature during the condensation reaction is 10-50° C. and the pressure is 0.2-0.3 MPa.
[0019] Compared with the prior art, the advantages and positive effects of the present invention are:
[0020] The catalyst provided by the present invention has a suitable void structure, strong mechanical properties, improved active site dispersion, and increased catalyst service life. At the same time, the addition of one or more elements of lanthanum, germanium, and zirconium in the catalyst helps to improve the catalytic efficiency of the catalyst and inhibit the generation of by-products. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The invention provides a catalyst for acetaldehyde condensation reaction, comprising a carrier, an active component and a catalyst promoter; the active component is magnesium oxide; the catalyst promoter is one or more of lanthanum, germanium and zirconium; the carrier is prepared from magnesium salt and aluminum salt, and chitosan and / or glucose is added during the preparation of the carrier.
[0023] In the present invention, the molar ratio of magnesium and aluminum elements in the magnesium salt and aluminum salt is 1:1-4. In the present invention, the addition amount of chitosan and / or glucose is 10%-20% of the total mass of the magnesium salt and aluminum salt. In the present invention, the molar ratio of the magnesium salt to the catalyst promoter is 1:0.02-0.06. In the present invention, the magnesium salt is one or more of magnesium citrate, magnesium nitrate and magnesium acetate; the aluminum salt is aluminum nitrate and / or aluminum citrate.
[0024] The catalyst for acetaldehyde condensation reaction provided by the present invention uses magnesium salt and aluminum salt to prepare a carrier. The magnesium salt serves as both a carrier and an active component, and can form a water-resistant framework structure and play a catalytic role. Chitosan and / or glucose are added during the preparation process. During the roasting process, organic matter generates carbon dioxide in an oxygen-containing atmosphere, which increases the porosity of the catalyst and is conducive to acetaldehyde molecules entering the pores to generate a catalytic reaction. Lanthanum, germanium and zirconium are added as catalyst additives to improve the selectivity of the catalyst.
[0025] The present invention provides a method for preparing the catalyst for acetaldehyde condensation reaction as described in any one of the above, comprising the following steps:
[0026] 1) mixing a magnesium salt solution, an aluminum salt solution, a chitosan and / or glucose solution, and an alkali solution to obtain a mixed solution;
[0027] 2) reacting, filtering, washing to neutrality and calcining the mixed solution in sequence to obtain a carrier with magnesium oxide as an active component;
[0028] 3) The precursor of the catalyst promoter is loaded onto the carrier, and the catalyst is obtained by sequentially standing, drying, calcining and tableting.
[0029] The present invention mixes a magnesium salt solution, an aluminum salt solution, a solution of chitosan and / or glucose, and an alkali solution to obtain a mixed solution. In the present invention, the alkali is preferably one or more of sodium hydroxide, potassium hydroxide, monoethanolamine and ammonia water; the amount of the alkali is preferably 1.2 to 2.2 times the sum of the amounts of magnesium and aluminum elements, and more preferably 1.3 to 1.5. In the present invention, the liquid inlet rates of the magnesium salt solution, the aluminum salt solution, the chitosan and / or glucose solution are independently preferably 0.5 mL / min-4 mL / min, and more preferably 1 mL / min-2 mL / min. In the present invention, the liquid inlet rate of the alkali solution is preferably 1 mL / min-5 mL / min, and more preferably 2 mL / min-4 mL / min. In the present invention, adding alkali solution during the preparation of the carrier is conducive to the precipitation of magnesium ions and aluminum ions in the solution.
[0030] After obtaining the mixed solution, the present invention sequentially reacts, filters, washes to neutrality and roasts the mixed solution to obtain a carrier with magnesium oxide as an active component. In the present invention, the temperature during the reaction is preferably 80-150°C, and the time is preferably 5-15h. In the present invention, deionized water is used to wash until the conductivity is ≤30us / cm, which is determined to be neutral. In the present invention, it is preferably dried before roasting. The drying temperature is preferably 60-140°C, more preferably 80°C-120°C; the time is preferably 6-24h, more preferably 12-18h. In the present invention, the roasting temperature is preferably 400-600°C, more preferably 150-550°C; the time is preferably 4-10h, more preferably 6-8h. The present invention adopts a precipitation method to prepare a catalyst carrier, which has the advantages of simple operation, low cost, and good purification effect.
[0031] After obtaining a carrier with magnesium oxide as an active component, the present invention loads the precursor of the catalyst promoter onto the carrier, and sequentially dries, calcines and tablets to obtain a catalyst. In the present invention, the precursor of the catalyst promoter is preferably one or more of lanthanum nitrate, zirconium nitrate and germanium nitrate. In the present invention, it is preferred to load the precursor of the catalyst promoter on the carrier by impregnation; the impregnation time is preferably 4 to 10 hours, more preferably 6 to 8 hours. The drying temperature is preferably 60 to 140°C, more preferably 80 to 120°C; the drying time is preferably 6 to 24 hours, more preferably 12 to 18 hours. The calcination temperature is preferably 400 to 600°C, more preferably 450 to 550°C; the calcination time is preferably 4 to 10 hours, more preferably 6 to 8 hours. In the present invention, after tableting, it is preferred that the particle size of the catalyst is 20 to 80 meshes, more preferably 25 to 40 meshes.
[0032] The present invention provides the use of any of the above-mentioned catalysts in the preparation of 3-hydroxybutyraldehyde by acetaldehyde condensation reaction, and the condensation reaction is carried out in a fixed bed. In the present invention, an acetaldehyde aqueous solution is used as a raw material, and the volume concentration of acetaldehyde in the acetaldehyde aqueous solution is preferably 20% to 80%, and more preferably 40% to 70%. In the present invention, the liquid inlet rate of the acetaldehyde aqueous solution is preferably 2mL / h to 10mL / h, and more preferably 3mL / h to 8mL / h. In the present invention, the reaction temperature during the condensation reaction is preferably 10 to 50°C, and the pressure is preferably 0.2 to 0.3Mpa. In the present invention, before the reaction, it is preferred to flush the pipeline with nitrogen, and nitrogen is always introduced during the reaction process, and the pressure in the reaction tube is controlled by regulating the amount of nitrogen introduced so that the pressure in the reaction tube is always maintained at 0.2 to 0.3Mpa.
[0033] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0034] Example 1
[0035] Weigh 59.326g of magnesium nitrate and dissolve it in 200mL of deionized water to form liquid A, weigh 170.396g of aluminum nitrate and dissolve it in 200mL of deionized water to form liquid B, weigh 42g of chitosan and dissolve it in 100mL of hydrochloric acid solution with a mass concentration of 1% to form liquid C, and weigh 63.09g of ammonia water as liquid D. Liquid A, liquid B, liquid C and liquid D were mixed in a three-necked flask containing 50mL of deionized water at a rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. After mixing, the mixed solution was transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 100℃ for 10h. After the autoclave was cooled to room temperature, the mixed solution was filtered and the filter cake was washed with deionized water until the washing liquid was neutral (conductivity ≤30us / cm). The filter cake was placed in a watch glass and dried in an oven at 110℃ for 12h. After drying, put it in a crucible and roast it at 550℃ for 6h to obtain a carrier. Weigh 1.677g of germanium nitrate and 1.677g of lanthanum nitrate, dissolve them in 16.775mL of deionized water, and immerse equal volumes in the prepared carrier (immerse at 25℃ for 6h). After impregnation, dry it at 100℃ for 12h. After drying, roast it at 500℃ for 6h. Press the prepared catalyst into tablets, screen the catalyst with 20-40 mesh, and record it as catalyst 1.
[0036] Example 2
[0037] Weigh 59.326g of magnesium nitrate and dissolve it in 200mL of deionized water to form liquid A, weigh 170.396g of aluminum citrate and dissolve it in 200mL of deionized water to form liquid B, weigh 36.032g of glucose and dissolve it in 100mL of deionized water to form liquid C, and weigh 63.09g of ammonia water as liquid D. Liquid A, liquid B, liquid C and liquid D flow into a three-necked flask containing 50mL of deionized water at a flow rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. The mixed solution is transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 150℃ for 5h. After the autoclave is cooled to room temperature, the mixed solution is filtered and the filter cake is washed with deionized water until the washing liquid is neutral (conductivity ≤30us / cm). The filter cake is placed in a watch glass and dried in an oven at 140℃ for 6h. After drying, put it in a crucible and roast it at 550℃ for 6h to obtain a carrier. Weigh 1.667g of germanium nitrate and 1.667g of lanthanum nitrate, dissolve them in 16.775mL of deionized water, and immerse equal volumes in the prepared carrier, immerse at 25℃ for 4h, and then dry at 60℃ for 24h. After drying, roast it at 600℃ for 4h. Press the prepared catalyst into tablets, screen the catalyst with 20-40 mesh, and record it as catalyst 2.
[0038] Example 3
[0039] Weigh 56.956g of magnesium acetate and dissolve it in 200mL of deionized water to form liquid A, weigh 172.864g of aluminum citrate and dissolve it in 200mL of deionized water to form liquid B, weigh 36.032g of glucose and dissolve it in 100mL of deionized water to form liquid C, and weigh 72g of sodium hydroxide and dissolve it in 100mL of deionized water to form liquid D. Liquid A, liquid B, liquid C and liquid D flow into a three-necked flask containing 50mL of deionized water at a rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. The mixed solution is transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 100℃ for 10h. After the autoclave is cooled to room temperature, the mixed solution is filtered and the filter cake is washed with deionized water until the washing liquid is neutral (conductivity ≤30us / cm). The filter cake is placed in a watch glass and dried in an oven at 110℃ for 12h. After drying, put it in a crucible and roast it at 400℃ for 10h to obtain a carrier. Then weigh 1.667g germanium nitrate, 1.667g lanthanum nitrate, and 1.667g zirconium nitrate, dissolve them in 16.775mL deionized water, and immerse equal volumes in the prepared carrier. Immerse at 25℃ for 4h, dry at 140℃ for 12h after impregnation, and roast at 400℃ for 10h after drying. Press the prepared catalyst into tablets, screen the catalyst with 20-40 mesh, and record it as catalyst 3.
[0040] Example 4
[0041] Weigh 56.956g of magnesium acetate and dissolve it in 200mL of deionized water to form liquid A, weigh 172.864g of aluminum citrate and dissolve it in 200mL of deionized water to form liquid B, weigh 36.032g of glucose and dissolve it in 100mL of deionized water to form liquid C, and weigh 72g of sodium hydroxide and dissolve it in 100mL of deionized water to form liquid D. Liquid A, liquid B, liquid C and liquid D flow into a three-necked flask containing 50mL of deionized water at a rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. The mixed solution is transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 100℃ for 10h. After the autoclave is cooled to room temperature, the mixed solution is filtered and the filter cake is washed with deionized water until the washing liquid is neutral (conductivity ≤30us / cm). The filter cake is placed in a watch glass and dried in an oven at 110℃ for 12h. After drying, put it in a crucible and roast it at 550℃ for 6h to obtain a carrier. Then weigh 1.667g of germanium nitrate and 1.667g of lanthanum nitrate, dissolve them in 16.775mL of deionized water, and immerse equal volumes in the prepared carrier for 6h at 25℃. After impregnation, dry it at 100℃ for 12h. After drying, roast the catalyst at 500℃ for 6h. Press the prepared catalyst into tablets, screen the catalyst with 20-40 mesh, and record it as catalyst 4.
[0042] Example 5
[0043] Weigh 56.956g of magnesium acetate and dissolve it in 200mL of deionized water to form liquid A, weigh 172.864g of aluminum citrate and dissolve it in 200mL of deionized water to form liquid B, weigh 36.032g of glucose and dissolve it in 100mL of deionized water to form liquid C, and weigh 72g of sodium hydroxide and dissolve it in 100mL of deionized water to form liquid D. Liquid A, liquid B, liquid C and liquid D flow into a three-necked flask containing 50mL of deionized water at a rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. The mixed solution is transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 100℃ for 10h. After the autoclave is cooled to room temperature, the mixed solution is filtered and the filter cake is washed with deionized water until the washing liquid is neutral (conductivity ≤30us / cm). The filter cake is placed in a watch glass and dried in an oven at 110℃ for 12h. After drying, put it in a crucible and roast it at 550℃ for 6h to obtain a carrier. Then weigh 3.355g of germanium nitrate, dissolve it in 16.775mL of deionized water, and immerse an equal volume in the prepared carrier for 6h at 25℃. After impregnation, dry it at 100℃ for 12h. After drying, roast the catalyst at 500℃ for 6h. Press the prepared catalyst into tablets, screen the catalyst with 20-40 mesh, and record it as catalyst 5.
[0044] Example 6
[0045] Weigh 56.956g of magnesium acetate and dissolve it in 200mL of deionized water to form liquid A, weigh 172.864g of aluminum citrate and dissolve it in 200mL of deionized water to form liquid B, weigh 36.032g of glucose and dissolve it in 50mL of deionized water to form liquid C, and weigh 72g of sodium hydroxide and dissolve it in 100mL of deionized water to form liquid D. Liquid A, liquid B, liquid C and liquid D flow into a three-necked flask containing 50mL of deionized water at a rate of 1mL / min, 1mL / min, 1mL / min, and 1.5mL / min, respectively. The mixed solution is transferred to an autoclave with a polytetrafluoroethylene liner and reacted at 100℃ for 10h. After the autoclave is cooled to room temperature, the mixed solution is filtered and the filter cake is washed with deionized water until the washing liquid is neutral (conductivity ≤30us / cm). The filter cake is placed in a watch glass and dried in an oven at 110℃ for 12h. After drying, put it in a crucible and roast it at 550℃ for 6h to obtain a carrier. Weigh 3.355g of lanthanum nitrate, dissolve it in 16.775mL of deionized water, and immerse an equal volume in the prepared carrier for 6h at 25℃. After impregnation, dry it at 100℃ for 12h, and after drying, roast it at 500℃ for 6h. Press the prepared catalyst into tablets, and select the catalyst with 20-40 mesh, which is recorded as catalyst 6.
[0046] Comparative Example 1
[0047] The difference from Example 1 is that chitosan is not added during the carrier preparation process, and the other operating steps are exactly the same as Example 1. The prepared catalyst is recorded as Catalyst 7.
[0048] Comparative Example 2
[0049] The difference from Example 1 is that fructose is used to replace chitosan in the carrier preparation process, and the other operation steps are exactly the same as those of Example 1. The prepared catalyst is recorded as Catalyst 8.
[0050] Comparative Example 3
[0051] The difference from Example 1 is that no catalyst aid is added during the preparation process, and the other operation steps are exactly the same as those of Example 1. The prepared catalyst is recorded as Catalyst 9.
[0052] Comparative Example 4
[0053] The difference from Example 1 is that no aluminum nitrate solution is added during the carrier preparation process, and the other operation steps are exactly the same as those of Example 1. The prepared catalyst is recorded as Catalyst 10.
[0054] Example 7
[0055] The catalysts prepared in the embodiment and the comparative example were used to catalyze the condensation of acetaldehyde. The specific reaction process was as follows: the reactor was a stainless steel tubular reactor of φ10mm×400mm, the bottom and top of the catalyst were filled with quartz sand and quartz wool, and the middle was filled with 5g of catalyst. The reaction temperature was 30°C, the reaction material was an aqueous solution of acetaldehyde with a volume concentration of 50%, and the feed rate of the reactant was 5mL / h. Before the reaction started, the pipeline was purged with nitrogen at 100mL / min to maintain the pressure of the reaction tube at 0.2Mpa. At the beginning of the reaction, the feed rate of nitrogen was 10mL / min to maintain the pressure of the reaction system at 0.2Mpa. The specific results are shown in Table 1.
[0056] Table 1
[0057]
[0058] It can be seen from Table 1 that in the catalyst preparation process, adding chitosan / glucose and adding lanthanum nitrate, germanium nitrate and zirconium nitrate as additives are more conducive to the conversion of acetaldehyde into 3-hydroxybutyraldehyde.
[0059] Comparative Example 5
[0060] Add 2 mL of 1% sodium hydroxide to 30 mL of acetaldehyde, and react at 0°C for 10 min. Then add 0.8% acetic acid solution until the pH of the solution is 7. The conversion rate of acetaldehyde is 50.23%, the selectivity of 3-hydroxybutyraldehyde is 78.16%, and the yield of 3-hydroxybutyraldehyde is 39.25%.
[0061] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A catalyst for acetaldehyde condensation reaction, characterized in that: The invention comprises a carrier, an active component and a catalyst promoter; the active component is magnesium oxide; the catalyst promoter is one or more of lanthanum, germanium and zirconium; the carrier is prepared from magnesium salt and aluminum salt, and chitosan and / or glucose are added during the preparation of the carrier; The molar ratio of magnesium to aluminum in the magnesium salt and aluminum salt is 1:1-4; the amount of chitosan and / or glucose added is 10%-20% of the total mass of the magnesium salt and aluminum salt; the molar ratio of the magnesium salt to the catalyst additive is 1:0.02-0.06; The magnesium salt is one or more of magnesium citrate, magnesium nitrate and magnesium acetate; the aluminum salt is aluminum nitrate and / or aluminum citrate; The method for preparing the catalyst for acetaldehyde condensation reaction comprises the following steps: 1) mixing a magnesium salt solution, an aluminum salt solution, a chitosan and / or glucose solution, and an alkali solution to obtain a mixed solution; 2) reacting, filtering, washing to neutrality and calcining the mixed solution in sequence to obtain a carrier with magnesium oxide as an active component; 3) The precursor of the catalyst promoter is loaded onto the carrier, and the catalyst is obtained by drying, calcining and tableting in sequence; The precursor of the catalyst promoter is one or more of lanthanum nitrate, zirconium nitrate and germanium nitrate.
2. The method for preparing the catalyst for acetaldehyde condensation reaction according to claim 1, characterized in that: The steps include: 1) mixing a magnesium salt solution, an aluminum salt solution, a chitosan and / or glucose solution, and an alkali solution to obtain a mixed solution; 2) reacting, filtering, washing to neutrality and calcining the mixed solution in sequence to obtain a carrier with magnesium oxide as an active component; 3) The precursor of the catalyst promoter is loaded onto the carrier, and the catalyst is obtained by drying, calcining and tableting in sequence; The precursor of the catalyst promoter is one or more of lanthanum nitrate, zirconium nitrate and germanium nitrate.
3. The preparation method according to claim 2, characterized in that: In step 1), the base is one or more of sodium hydroxide, potassium hydroxide, monoethanolamine and ammonia water; the amount of the base is 1.2 to 2.2 times the sum of the molar amounts of magnesium and aluminum elements.
4. The preparation method according to claim 2, characterized in that: In step 2), the reaction temperature is 80-150° C. and the reaction time is 5-15 hours; the calcination temperature is 400-600° C. and the reaction time is 4-10 hours.
5. The preparation method according to claim 2, characterized in that: In step 3), the precursor of the catalyst promoter is loaded on the carrier by impregnation; the impregnation time is 4 to 10 hours.
6. The preparation method according to claim 2, characterized in that: In step 3), the drying temperature is 60-140° C., and the time is 6-24 hours; the calcination temperature is 400-600° C., and the time is 4-10 hours.
7. Use of the catalyst according to claim 1 in the preparation of 3-hydroxybutyraldehyde by acetaldehyde condensation reaction, characterized in that: A fixed bed was used for the condensation reaction.
8. The use according to claim 7, characterized in that: The reaction temperature during the condensation reaction is 10~50°C and the pressure is 0.2~0.3Mpa.