A microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked together, and its preparation method and application
By preparing microspheres composed of ordered cobalt-manganese bimetallic nanoparticle sheets, the problems of easy aggregation of cobalt-based nanoparticles and leaching of cobalt ions were solved, and efficient catalytic activation of persulfate to oxidize and degrade organic micropollutants in water was achieved, which has broad prospects for practical application.
Patent Information
- Application Number
- CN202411075877.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing cobalt-based nanoparticle materials are prone to agglomeration and cobalt ion leaching during the catalytic activation of persulfate, which affects the removal efficiency of organic micropollutants in water, and their structural stability is insufficient.
Microspheres composed of ordered cobalt-manganese bimetallic nanoparticle sheets were prepared by a hydrothermal-sacrificial template method, forming an ordered microsphere structure that enhances the synergistic effect between particles, restricts cobalt ion leaching, and improves catalytic activity.
This study improves the stability and catalytic activity of cobalt-manganese bimetallic nanoparticles, reduces the risk of cobalt ion leaching, enhances the oxidative degradation efficiency of organic micropollutants, has a wide applicable pH range, low cost, and is environmentally friendly.
Smart Images

Figure CN118594626B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of environmental functional materials, and in particular to a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked together, and a preparation method and application thereof. Background Art
[0002] Sulfate radical (SO4 ·- )-mediated advanced oxidation technology can deeply mineralize organic micropollutants in water, so this technology has received widespread attention in the field of water pollution control. Permonosulfate (PMS) is a solid-phase oxidant with more stable physical and chemical properties than hydrogen peroxide. As a precursor, it can produce a large number of sulfate radicals through activation pathways. In addition, most studies have shown that cobalt-based materials are more suitable as PMS activators under low energy consumption requirements. However, traditional cobalt-based materials are affected by reaction factors (such as pH, inorganic anions, temperature), cobalt ion leaching, particle agglomeration and other issues during the PMS activation process. Cobalt ion leaching can cause secondary pollution of water bodies, and particle agglomeration will accelerate the passivation of the activator and directly affect the removal effect of organic micropollutants in water. Therefore, the simultaneous guarantee of the catalytic activity and structural stability of cobalt-based materials is not only a necessary prerequisite for improving their practical engineering application potential, but also a technical problem that urgently needs to be overcome.
[0003] Nanoscale materials can exhibit excellent catalytic performance due to their large specific surface area and high mass transfer efficiency. However, due to their inherent magnetic characteristics, cobalt-based materials in nanoparticle form cannot overcome the magnetic attraction that easily leads to agglomeration. In terms of improving catalytic activity, manganese is doped into the cobalt tetroxide lattice. The potential difference between the two promotes charge transfer and helps alleviate the passivation of catalytic active sites. However, the mismatch of electrons outside the nucleus can easily cause structural defects in cobalt-manganese bimetallic materials, limiting their stability in engineering applications. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle layers stacked together, and a preparation method and application thereof, so as to solve the problems of easy agglomeration of existing cobalt-based nanoparticles and the risk of cobalt ion leaching.
[0005] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:
[0006] On the one hand, a method for preparing a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked together is provided, which comprises the following steps:
[0007] (1) Dissolve KIT-6 in anhydrous ethanol at room temperature, slowly add Co(NO3)2·6H2O and MnCl2 and stir until completely dissolved;
[0008] (2) heating the solution, cooling it to room temperature, centrifuging, washing and drying the reaction mixture in sequence, and then calcining it at high temperature;
[0009] (3) The powder after high-temperature calcination is placed in a NaOH solution, stirred continuously in a water bath atmosphere, and then washed with distilled water until the washing liquid is neutral. The dried powder is then reduced with NaBH4 to obtain a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked together.
[0010] Furthermore, in step (1), the molar mass ratio of Co(NO3)2·6H2O and MnCl2 is 2:1.
[0011] Furthermore, step (1) uses magnetic stirring, the magnetic stirring time is 1 hour, and the magnetic stirring speed is 200-250 rpm.
[0012] Furthermore, step (2) is subjected to heating treatment in a high-pressure hydrothermal reactor containing a polytetrafluoroethylene liner, the hydrothermal reaction temperature is 200° C., and the hydrothermal reaction duration is 6 hours.
[0013] Furthermore, in step (2), the calcination temperature is 450°C, the calcination duration is 6 hours, and the heating rate is 5°C / min.
[0014] Furthermore, in step (3), the water bath temperature is 80° C., and the stirring time in the water bath is continuous for 12 h.
[0015] Furthermore, the drying temperature in step (3) is 60° C., and the drying treatment duration is 12 hours.
[0016] On the other hand, a microsphere material composed of stacked cobalt-manganese bimetallic ordered nanoparticle sheets is provided as a catalyst for catalytic activation of peroxymonosulfate to oxidatively degrade organic micropollutants in water.
[0017] Furthermore, the organic micropollutants are at least one of ranitidine, rhodamine B, methyl orange, methylene blue, ciprofloxacin, norfloxacin, bisphenol A and tetracycline hydrochloride.
[0018] The beneficial effects of the present invention are:
[0019] (1) The present invention provides for the first time a method for preparing RNS MnCo2O4, which has low requirements for synthesis equipment, low investment cost, and is convenient for batch processing under industrial promotion;
[0020] (2) The RNS MnCo2O4 synthesized in the present invention is in the form of microspheres composed of arranged cobalt-manganese bimetallic nanoparticles, and the interparticle mesopores provide channels for the active sites inside the microspheres to improve the overall catalytic performance;
[0021] (3) The ordered arrangement of the ordered cobalt-manganese bimetallic nanoparticles in the RNS MnCo2O4 synthesized by the present invention can improve the synergistic effect between the particles to overcome the particle agglomeration problem caused by magnetic attraction and limit the leaching of cobalt ions;
[0022] (4) The material synthesized by the present invention can trigger rapid charge transfer between dual active sites, enhance the catalytic activity of PMS, and has the ability to rapidly oxidize and degrade organic micropollutants, and has great practical potential;
[0023] (5) The material synthesized by the present invention has good reusability, is environmentally friendly, is applicable to a wide pH range, has strong impact load resistance, and can reduce the risk of secondary pollution caused by cobalt ion leaching;
[0024] (6) The material preparation method of the present invention does not require the consumption of additional energy, thus reducing the operating cost; in addition, the process is simple, the operability is strong, the material usage is small and the durability is good, the treatment time is short, and it has broad practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The X-ray crystal diffraction pattern (XRD) of the microsphere material RNSMNCo2O4 composed of the stacked layers of cobalt-manganese bimetallic ordered nanoparticles prepared in Example 1;
[0026] Figure 2 In the figure, a, b, c and d are scanning electron microscope images (SEM) of the microsphere material RNS MnCo2O4 composed of the cobalt-manganese bimetallic ordered nanoparticle sheets prepared in Example 1 at different magnifications; e is a scanning electron microscope transmission image (STEM), and f, g and h are X-ray energy dispersion spectra (EDS) of oxygen, manganese and cobalt elements;
[0027] Figure 3 In the figure, a and b are X-ray photoelectron spectra (XPS) of manganese and cobalt elements on the microsphere material RNS MnCo2O4 composed of the stacked cobalt-manganese bimetallic ordered nanoparticle sheets prepared in Example 1;
[0028] Figure 4 Comparison of the leaching concentrations of cobalt and manganese ions between RNS MnCo2O4 and commercial grade MnCo2O4 materials in Example 3;
[0029] Figure 5 It is the type of active oxidative species in the process of RNS MnCo2O4 catalytic activation of PMS oxidative degradation of RAN in Example 4. DETAILED DESCRIPTION
[0030] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.
[0031] In this example, ranitidine (RAN) is used as the target pollutant. In order to demonstrate the effectiveness of the present invention in the pollution control of typical organic pollutants, rhodamine B (RhB), methyl orange (MO), methylene blue (MB), ciprofloxacin (CIF), norfloxacin (NOF), bisphenol A (BPA) and tetracycline hydrochloride (TC) are also selected as research objects.
[0032] Embodiment 1:
[0033] This example compares the effect of RNS MnCo2O4 catalytic activation of PMS on oxidative degradation of different organic micropollutants (RAN, RhB, MO, MB, CIF, NOF, BPA, TC).
[0034] (1) Preparation of RNS MnCo2O4: At room temperature, 0.5 g of KIT-6 was dissolved in a 50 mL beaker containing 10 mL of anhydrous ethanol under the assistance of ultrasound (ultrasonic frequency of 20 kHz, duration of 10 min), and then Co(NO3)2·6H2O (0.8 M) and MnCl2 (0.4 M) were slowly added and magnetic stirring (speed of 250 rpm) was continued for 1 h until it was completely dissolved. The above solution was placed in a 100 mL high pressure hydrothermal reactor with a polytetrafluoroethylene liner and heated at 200 °C for 6 h. After cooling to room temperature (25 °C), the reaction mixture was centrifuged at 10,000 rpm for 15 min to achieve solid-liquid separation, washed three times with deionized water and anhydrous ethanol respectively, dried in a forced air drying oven at 60 °C for 6 h, and then calcined at 450 °C for 6 h. The above powder was placed in 100 mL of NaOH (8 g) solution and stirred continuously for 6 h in a water bath at 80 °C. Then it was washed with distilled water until the washing solution was neutral, that is, the pH of the washing solution was close to 6.5-7.5. After the powder was dried at 60 °C in vacuum for 12 h, 3.8 g of NaBH4 was added for reduction treatment, which was a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked, marked as RNS MnCo2O4.
[0035] The XRD, SEM / STEM-EDS and XPS spectra of the prepared RNS MnCo2O4 are shown in Figure 1 , 2, 3. Among them, the microsphere structure can be observed through SEM / STEM images, and the cobalt and manganese dual active sites are densely and evenly distributed on the surface of RNSMNCo2O4.
[0036] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0037] (3) A 200 mL beaker with a lid was used as a reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption saturation was reached. Then 10.0 mg of PMS was added into the reactor. The temperature was controlled at 25 °C in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points for analysis.
[0038] (4) Add 5 mg / L rhodamine B (RhB) to the reactor to replace ranitidine (RAN). Other conditions are the same as (3).
[0039] (5) Add 5 mg / L methyl orange (MO) to the reactor instead of ranitidine (RAN). Other conditions are the same as (3).
[0040] (6) Add 5 mg / L methylene blue (MB) to the reactor instead of ranitidine (RAN). Other conditions are the same as (3).
[0041] (7) Add 5 mg / L ciprofloxacin (CIF) to the reactor instead of ranitidine (RAN). Other conditions are the same as (3).
[0042] (8) Add 5 mg / L norfloxacin (NOF) to the reactor instead of ranitidine (RAN). Other conditions are the same as (3).
[0043] (9) Add 5 mg / L bisphenol A (BPA) to the reactor to replace ranitidine (RAN). Other conditions are the same as (3).
[0044] (10) Add 5 mg / L tetracycline hydrochloride (TC) to the reactor instead of ranitidine (RAN). Other conditions are the same as (3).
[0045] After 10 minutes of catalytic oxidation reaction, the removal effects of different organic micropollutants are shown in Table 1.
[0046] Table 1 Removal rates of different organic micro-pollutants
[0047]
[0048] It can be seen from Table 1 that in the process of catalytic activation of PMS by RNS MnCo2O4, the removal rates of different types of organic micropollutants were all above 89.0%. The efficient removal of typical organic micropollutants in water is closely related to the excellent catalytic activity exerted by the characteristic structure of the prepared RNS MnCo2O4, and it is sufficient to show that the constructed PMS-mediated advanced oxidation process can achieve the pollution control effect of organic micropollutants in water.
[0049] Embodiment 2:
[0050] In this example, the ranitidine (RAN) selected in Example 1 can achieve an ideal removal effect within a reaction time of 10 minutes, so it can be used as a target pollutant. This example compares the efficiency of RNS MnCo2O4 prepared in Example 1 and different oxidation technologies in catalyzing the activation of PMS to degrade RAN.
[0051] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0052] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0053] (3) A 200 mL beaker with a lid was used as a reactor, into which 200 mL of RAN solution and 5.0 mg (RNSMnCo2O4, MoS2 / rGO, MoS2, rGO, MXene-Ti3C2 / MoS2, TiO2, TiO2+ Fe 2+ or NH2Cl), adjust the initial pH value of the solution (pH=7.0), and let it stand for 2 minutes to reach adsorption saturation. Then add 10.0 mg PMS, and carry out magnetic stirring (speed 250 rpm) at a controlled temperature (25°C) in a water bath, and take samples at fixed points for analysis.
[0054] (4) Using the most scientific reaction kinetics formula (1-1), the reaction rates (k) of different oxidation technologies were calculated and compared to evaluate the RAN oxidation degradation efficiency.
[0055] k = 1 / m × dC RAN / dt (1-1)
[0056] Where k is the reaction rate, m is the catalyst dosage, C RAN is the RAN concentration, and t is the reaction time.
[0057] The comparison of RAN removal efficiency of different oxidation technologies is shown in Table 2.
[0058] Table 2 Comparison of RAN removal efficiency evaluation of different oxidation technologies
[0059]
[0060] It can be seen from Table 2 that the reaction rate constant calculated by formula (1-1) directly expresses the treatment efficiency of the oxidation technology. By comparing with the existing research oxidation process, the RNS MnCo2O4 prepared by the present invention has significant advantages in the efficiency of oxidative degradation of RAN by catalytic activation of PMS. Under the condition of ensuring a high removal rate of RAN, the material usage is minimal, the operation time is short, and no additional energy input is required, which better meets the current technical requirements for RAN pollution control in water. The reaction rate constant of oxidative degradation of RAN by catalytic activation of PMS by RNS MnCo2O4 prepared by the present invention is 2.37 to 2886.16 times that of the above-mentioned oxidation technology, indicating that the modified material has the ability of rapid oxidation degradation and great practical potential.
[0061] Embodiment 3:
[0062] Through Example 1 and Example 2, it is verified that the RNS MnCo2O4 prepared by the present invention has the characteristics of strong practicality, but the high risk of ion leaching is also a key problem limiting this technology. In this example, ICP-OES / MS is used to detect and compare the ion leaching concentration of RNS MnCo2O4 and commercial grade MnCo2O4 materials.
[0063] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0064] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0065] (3) A 200 mL beaker with a lid was used as a reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption saturation was reached. Then 10.0 mg of PMS was added into the reactor. The temperature (25 °C) was controlled in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points. The concentrations of cobalt and manganese ions leached in the solution were analyzed and detected using an Agilent 5110 ICP-OES / MS.
[0066] (4) Add 5.0 mg of commercial grade MnCo2O4 material to the beaker to replace RNS MnCo2O4. Other conditions are the same as (3).
[0067] The leaching concentrations of cobalt and manganese ions of RNS MnCo2O4 and commercial grade MnCo2O4 materials were tested. The results are shown in Table 3 and Figure 4 shown.
[0068] Table 3 Cobalt and manganese ion leaching concentrations
[0069]
[0070] From Table 3 and Figure 4 It can be seen that in the catalytic oxidation experiment with a reaction time of 10 minutes, ICP-OES / MS was used to detect the leaching concentrations of cobalt and manganese ions in RNS MnCo2O4 and commercial-grade MnCo2O4 materials. Compared with commercial-grade MnCo2O4 materials, the leaching concentrations of cobalt and manganese ions in RNS MnCo2O4 were reduced to 0.15 times and 0.25 times of those in commercial-grade MnCo2O4 materials, respectively, indicating that the RNS MnCo2O4 prepared by the present invention is an environmentally friendly material and effectively reduces the risk of secondary water pollution caused by ion leaching. Figure 2 As shown in b, the surface of the RNS MnCo2O4 prepared by the present invention is composed of orderly arranged cobalt-manganese bimetallic nanoparticles, which can effectively bind free cobalt and manganese ions by enhancing the synergistic effect between particles, so as to reduce the risk of ion leaching.
[0071] Embodiment 4:
[0072] In this example, 5,5-dimethyl-1-pyrrolidine-N-oxide (DMPO) and 2,2,6,6-tetramethylpiperidine (TEMP) were used as free radical scavengers to conduct electron spin resonance (EPR) experiments to determine the types of active oxidative species in the process of RNS MnCo2O4 catalytic activation of PMS for oxidative degradation of RAN.
[0073] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0074] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0075] (3) A 200 mL beaker with a lid was used as a reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added to the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption reached saturation. Then 10.0 mg of PMS was added to the reactor. The temperature was controlled at 25 °C in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at a fixed point. 50 μL of DMPO / TEMP aqueous solution was added. After mixing evenly, the mixture was aspirated with a capillary. The mixture was then covered with a quartz tube and placed in the EPR (BrukerEMXplus-6 / 1, Germany) sample chamber for measurement.
[0076] Determination of the types of active oxidative species in the process of RAN degradation by PMS activated by RNS MnCo2O4 Figure 5 shown.
[0077] Depend on Figure 5It can be seen that in the process of RNS MnCo2O4 catalytic activation of PMS oxidation degradation of RAN, DMPO-SO4 can be captured by EPR. •− , DMPO-•OH and TEMP- 1 The corresponding signals of O2 indicate that the RNS MnCo2O4 prepared by the present invention can stimulate multiple free radical-mediated oxidation mechanisms and achieve rapid degradation of typical organic micropollutants in water.
[0078] Embodiment 5:
[0079] This example compares the effects of different pH values (pH=4.0, pH=5.0, pH=6.0, pH=7.0, pH=8.0, pH=9.0, pH=10.0) on the catalytic activation of PMS by RNS MnCo2O4 to oxidatively degrade RAN.
[0080] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0081] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0082] (3) A 200 mL beaker with a lid was used as the reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted (pH=4.0, pH=5.0, pH=6.0, pH=7.0, pH=8.0, pH=9.0, pH=10.0). After standing for 2 minutes, the adsorption reached saturation. Then, 10.0 mg of PMS was added into the reactor. The temperature (25°C) was controlled in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points for analysis.
[0083] The removal efficiency of RAN oxidative degradation by RNS MnCo2O4 catalytic activation of PMS at different initial pH values is shown in Table 4.
[0084] Table 4 RAN removal rate at different initial pH values
[0085]
[0086] As shown in Table 4, in the catalytic oxidation experiment with a reaction time of 10 minutes, under different initial pH conditions, the removal rate of RAN degradation by catalytic activation of PMS by RNS MnCo2O4 prepared by the present invention is above 94%, and the material can exert high RAN removal efficiency under acid and alkaline conditions. Therefore, the RNS MnCo2O4 prepared by the present invention can effectively catalytically activate PMS in a wide range of pH values (4.0 ~ 10.0) to quickly oxidize and degrade RAN in water, and has strong practicality.
[0087] Embodiment 6:
[0088] This example compares the effects of different water bath reaction temperatures (10°C, 15°C, 20°C, 25°C, 30°C) on the catalytic activation of PMS by RNS MnCo2O4 to oxidatively degrade RAN.
[0089] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0090] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0091] (3) A 200 mL beaker with a lid was used as the reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption saturation was reached. Then 10.0 mg of PMS was added into the reactor. The temperature was controlled in a water bath (10°C, 15°C, 20°C, 25°C, 30°C) and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points for analysis.
[0092] The removal rates of RAN oxidative degradation by RNS MnCo2O4 catalytic activation of PMS at different reaction temperatures are shown in Table 5.
[0093] Table 5 RAN removal rate at different reaction temperatures
[0094]
[0095] As can be seen from Table 5, at different water bath reaction temperatures, in the catalytic oxidation experiment with a reaction time of 10 minutes, the removal rate of RAN degradation by catalytic activation of PMS by RNS MnCo2O4 prepared by the present invention is above 90%. Therefore, the applicable temperature of the material meets the technical requirements of the natural water environment and my country's municipal water treatment system.
[0096] Embodiment 7:
[0097] This example compares the effects of different RNS MnCo2O4 dosages (1.0 mg, 3.0 mg, 5.0 mg, 7.0 mg) on the catalytic activation of PMS for oxidative degradation of RAN.
[0098] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0099] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0100] (3) A 200 mL beaker with a lid was used as a reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption saturation was reached. Then 10.0 mg of PMS was added into the reactor. The temperature was controlled at 25 °C in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points for analysis.
[0101] (4) Add 1.0 mg RNS MnCo2O4 into the beaker. Other conditions are the same as (3).
[0102] (5) Add 3.0 mg RNS MnCo2O4 into the beaker. Other conditions are the same as (3).
[0103] (6) Add 7.0 mg RNS MnCo2O4 into the beaker. Other conditions are the same as (3).
[0104] The removal efficiency of RAN oxidative degradation by catalytically activated PMS at different RNS MnCo2O4 dosages is shown in Table 6.
[0105] Table 6 RAN removal rate under different RNS MnCo2O4 dosage conditions
[0106]
[0107] As shown in Table 6, in the catalytic oxidation experiment with a reaction time of 10 minutes, the RAN removal rate increases with the increase in the dosage of RNSMNCo2O4 prepared by the present invention. When the dosage reaches 3.0 mg, the RAN removal rate can reach more than 95%. In actual engineering applications, the process treatment cost should be fully considered, and the most ideal RNSMNCo2O4 dosage for each 1L of water is 5.0 mg.
[0108] Embodiment 8:
[0109] This example compares different types of inorganic anions (such as Cl - 、H2PO4 - 、SO4 2- 、HPO4 - and NO3 - ) on the catalytic activation of PMS for oxidative degradation of RAN by RNSMNCo2O4.
[0110] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0111] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0112] (3) A 200 mL beaker with a lid was used as the reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption reached saturation. Then 10.0 mg of PMS was added. Different concentrations of NaCl (1 mM, 5 mM and 10 mM) were added. The solution was stirred magnetically (speed 250 rpm) at a controlled temperature (25 °C) in a water bath. Sampling was performed at fixed points for analysis.
[0113] (4) Add different concentrations (1mM, 5mM and 10mM) of NaH2PO4 to the beaker. Other conditions are the same as (3).
[0114] (5) Add different concentrations (1mM, 5mM and 10mM) of Na2SO4 into the beaker. Other conditions are the same as (3).
[0115] (6) Add different concentrations (1 mM, 5 mM and 10 mM) of NaHPO4 to the beaker. Other conditions are the same as (3).
[0116] (7) Add different concentrations (1mM, 5mM and 10mM) of NaNO3 into the beaker. Other conditions are the same as (3).
[0117] The removal rates of different types of inorganic anions on the oxidative degradation of RAN by RNS MnCo2O4-catalyzed activation of PMS are shown in Table 7.
[0118] Table 7 RAN removal rate under the conditions of adding different types of inorganic anions
[0119]
[0120] As shown in Table 7, in the catalytic oxidation experiment with a reaction time of 10 minutes, when different concentrations of common inorganic anions are added to the system, the removal rate of RAN oxidative degradation by catalytic activation of PMS prepared by the RNS MnCo2O4 of the present invention is still relatively high, indicating that the material has a strong ability to resist shock loads of substances in water.
[0121] Embodiment 9:
[0122] This example compares the recycling of RAN by oxidative degradation using RNS MnCo2O4 as the catalyst to activate PMS.
[0123] (1) The preparation of RNS MnCo2O4 is the same as step (1) in Example 1.
[0124] (2) Prepare a 5 mg / L ranitidine (RAN) solution for later use.
[0125] (3) A 200 mL beaker with a lid was used as a reactor. 200 mL of RAN solution and 5.0 mg of RNSMnCo2O4 were added into the reactor. The initial pH value of the solution was adjusted to 7.0. After standing for 2 minutes, the adsorption saturation was reached. Then 10.0 mg of PMS was added into the reactor. The temperature was controlled at 25 °C in a water bath and magnetic stirring (speed 250 rpm) was performed. Sampling was performed at fixed points for analysis.
[0126] (4) The RNS MnCo2O4 in the reaction solution of (3) was filtered out using a 0.1 mM sodium borohydride aqueous solution through an aqueous membrane with a pore size of 0.22 μm and then added to the reactor for the second time. Other conditions were the same as (3).
[0127] (5) The RNS MnCo2O4 in the reaction solution of (3) was filtered through an aqueous membrane with a pore size of 0.22 μm using a 0.1 mM sodium borohydride aqueous solution and added to the reactor for the third time. The other conditions were the same as (3).
[0128] (6) The RNS MnCo2O4 in the reaction solution of (3) was filtered out using a 0.1 mM sodium borohydride aqueous solution through an aqueous membrane with a pore size of 0.22 μm and added to the reactor for the fourth time. Other conditions were the same as (3).
[0129] (7) The RNS MnCo2O4 in the reaction solution of (3) was filtered through an aqueous membrane with a pore size of 0.22 μm using a 0.1 mM sodium borohydride aqueous solution and added to the reactor for the fifth time. Other conditions were the same as (3).
[0130] (8) The RNS MnCo2O4 in the reaction solution of (3) was filtered through an aqueous membrane with a pore size of 0.22 μm using a 0.1 mM sodium borohydride aqueous solution and added to the reactor for the sixth time. The other conditions were the same as (3).
[0131] (9) The RNS MnCo2O4 in the reaction solution of (3) was filtered through an aqueous membrane with a pore size of 0.22 μm using a 0.1 mM sodium borohydride aqueous solution and added to the reactor for the seventh time. The other conditions were the same as (3).
[0132] (10) The RNS MnCo2O4 in the reaction solution of (3) was filtered through an aqueous membrane with a pore size of 0.22 μm using a 0.1 mM sodium borohydride aqueous solution and added to the reactor for the eighth time. Other conditions were the same as (3).
[0133] The removal efficiency of RAN oxidative degradation by catalytically activated PMS at different RNS MnCo2O4 dosages is shown in Table 6.
[0134] Table 8 Recycling of RAN by catalytic activation of PMS by RNS MnCo2O4
[0135]
[0136] It can be seen from Table 8 that with the increase in the number of cycles, the removal rate of RAN oxidative degradation by catalytic activation of PMS by RNS MnCo2O4 shows a downward trend. The sodium borohydride aqueous solution treatment method proposed in the present invention can still ensure that the removal rate of RAN in the circulating water is higher than 60%. Verification tests show that this is mainly due to the passivation of the active sites on the surface of RNS MnCo2O4 and the loss of materials caused during the washing process. Compared with other commercial-grade materials, the material exhibits good durability and good reusability at a lower dosage. In addition, with the advantages of short treatment time, low risk of cobalt ion leaching in the effluent, and a wide applicable pH range, the RNS MnCo2O4 prepared by the present invention has broad practical application prospects.
[0137] In summary, the present invention adopts a hydrothermal-sacrificial template method to prepare a microsphere characteristic structure material composed of cobalt-manganese bimetallic ordered nanoparticles stacked on top of each other, which has a larger specific surface area and a higher density of dual catalytic active sites. The intergranular mesopores formed by the orderly arrangement of cobalt-manganese nanoparticles can provide a shuttle channel for the reaction molecules, improve the exposure rate of the catalytic active sites of the inner layer structure of the microspheres, and strengthen the synergistic effect between the cobalt-manganese bimetallic nanoparticles, which also helps to promote the charge transfer between the dual active sites and overcome the defects of ion leaching of traditional cobalt-based materials. The mesoporous channels between cobalt-manganese nanoparticles enable the catalytic active sites of the inner layer structure to participate in the reaction, and the stronger adsorption energy of cobalt ions by the mesoporous confinement reduces the risk of secondary pollution. Under the premise of simultaneously ensuring catalytic activity and structural stability, the operating cost of this environmentally friendly material has sufficient advantages, and it has great application prospects in the degradation of organic micropollutants in water.
[0138] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0139] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An application of a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked as a catalyst for catalytic activation of peroxymonosulfate to oxidatively degrade organic micropollutants in water, characterized in that: The method for preparing the microsphere material composed of stacked cobalt-manganese bimetallic ordered nanoparticle sheets comprises the following steps: (1) Dissolve KIT-6 in anhydrous ethanol at room temperature, slowly add Co(NO3)2·6H2O and MnCl2 and stir until completely dissolved; (2) heating the above solution in a high-pressure hydrothermal reactor containing a polytetrafluoroethylene liner, cooling to room temperature, centrifuging, washing and drying the reaction mixture in sequence, and then calcining at high temperature; (3) The powder after high-temperature calcination is placed in a NaOH solution, stirred continuously in a water bath atmosphere, and then washed with distilled water until the washing liquid is neutral. The dried powder is then reduced with NaBH4 to obtain a microsphere material composed of cobalt-manganese bimetallic ordered nanoparticle sheets stacked together.
2. The use according to claim 1, characterized in that: In step (1), the molar mass ratio of Co(NO3)2·6H2O to MnCl2 is 2:
1.
3. The use according to claim 1, characterized in that: Step (1) uses magnetic stirring, the magnetic stirring time is 1 hour, and the magnetic stirring speed is 200 ~ 250rpm.
4. The use according to claim 1, characterized in that: The heating treatment temperature in step (2) is 200° C. and the heating treatment duration is 6 hours.
5. The use according to claim 1, characterized in that: The calcination temperature in step (2) is 450°C, the calcination duration is 6 hours, and the heating rate is 5°C / min.
6. The use according to claim 1, characterized in that: The water bath temperature in step (3) is 80° C., and the stirring time in the water bath is 12 h.
7. The use according to claim 1, characterized in that: The drying temperature in step (3) is 60° C. and the drying treatment duration is 12 hours.
8. The use according to claim 1, characterized in that: The microsphere material has a diameter less than 3.5 μm, and the cobalt and manganese content accounts for more than 65 wt% of the total mass of the material.
9. The use according to claim 1, characterized in that: The organic micropollutant is at least one of ranitidine, rhodamine B, methyl orange, methylene blue, ciprofloxacin, norfloxacin, bisphenol A and tetracycline hydrochloride.